喷吹微粒脱磷法在130 t电弧炉炼钢中的应用

陈军召1,张彦辉2,谈岸童2,李立凯3,康建光2   

  1. 1中天钢铁集团有限公司,常州213000;
    2 新三洲特钢有限公司,无锡214181 ;
    3 东方特钢有限公司,常州213100
  • 收稿日期:2022-08-08 出版日期:2023-02-01 发布日期:2023-01-30
  • 通讯作者: 通讯作者:张彦辉(1960 -),男,工程师; E-mail: 18211161078® 163. com
  • 作者简介:作者简介:陈军召(1969 -),男,工程师;

Application of Particle Injection Dephosphorization Process on Steelmaking of 130 t Electric Arc Furnace

Chen Junzhao1, Zhang Yanhui2, Tan Antong2 , Li Likai3, Kang Jianguang2   

  1. 1 Zenith Steel Group Co., Ltd., Changzhou, 213000;
    2 Xinsanzhou Special Steel Co., Ltd., WuXi 214181 ;
    3 Eastran Special Steel Co., Ltd., ChangZhou 213100
  • Received:2022-08-08 Published:2023-02-01 Online:2023-01-30

摘要: 在130 t电弧炉上进行了复合喷吹剂喷吹微粒脱磷的实践应用。设计了电弧炉氧化期脱磷渣系的组成,炉渣碱度控制在2.2~2.8,氧化铁含量控制在15%~20%。并以氮气为载体喷吹按照一定比例配制的碳粉(15%~20%) 、CaO粉(40%~60%) 、MgO粉(25%~30%) 、CaC粉(5%~10%)的复合粉剂。40Cr、45钢、20CrMnTi和60Si2Mn等钢采用喷吹复合喷吹剂冶炼工艺后,加快了熔剂的反应面积,提高了成渣速度,各项生产指标得到了改善,其中吨钢电耗降低90 kWh/t,吨钢钢铁料消耗降低9.3 kg/t,吨钢熔剂消耗减少4.8 kg/t,生产率提高5%~6%,吨钢综合生产成本降低了25元/t。

关键词: 电弧炉, 脱磷, 喷吹, 复合粉剂, 成本

Abstract: The practical application of particle dephosphorization with compound injection agent on 130 t electric arc furnace is carried out. The composition of dephosphorization slag system in the oxidation period of electric furnace is designed, basicity of slag is controlled between 2.2-2. 8, and the content of iron oxide is controlled between 15% -20%. The composite powder of carbon powder (15% -20%), CaO powder (40% -60%), MgO powder (25% -30%) and CaC powder (5% - 10%) prepared in a certain proportion is injected with nitrogen as the carrier. After adopting the smelting process of injection compound injection agent on EAF steelmaking of 40Cr, 0.45C steel, 20CrMnTi and 60Si2Mn etc alloy steels, the reaction area of flux is accelerated, the slag forming speed is improved, and various production indexes are improved. Among them, the power consumption per ton steel is reduced by 90 kWh/t, the steel material consumption per ton steel is reduced by 9. 3 kg/t, the flux consumption per ton steel is reduced by 4. 8 kg/t, the productivity is increased by 5% -6%, and the comprehensive production cost per ton of steel is reduced by 25 yuan/t.

Key words: Electric Arc Furnace , Dephosphorization , Injection , Composite Powder , Cost