ISSN:1003-8620

CN:42-1243/TF

主管:中信泰富特钢集团股份有限公司

主办:大冶特殊钢有限公司

特殊钢 ›› 2013, Vol. 34 ›› Issue (6): 45-48.

• 组织和性能 • 上一篇    下一篇

定径和冷却工艺参数对40Mn2V钢N80-1套管组织和力学性能的影响

吴乐胜1,方剑1,2,李明新1,袁泽喜2   

  1. 1衡阳华菱钢管(集团)有限公司技术中心,衡阳421001;
    2武汉科技大学钢铁冶金及资源利用省部共建教育部重点实验室,武汉430081
  • 收稿日期:2013-05-13 出版日期:2013-12-01 发布日期:2022-09-07
  • 通讯作者: 方剑
  • 作者简介:吴乐胜(1969-),男,硕士,高级工程师,无缝钢管轧管工艺研发。

Influence of Sizing and Cooling Process on Structure and Mechanical Properties of N80-1 Seamless Casing Tube of Steel 40Mn2V

Wu Lesheng1, Fang Jian1,2, Li Mingxin1 ,Yuan Zexi2   

  1. 1 Technical Center, Hengyang Hualing Steel Tube (Group) Co Ltd, Hengyang 421001 ;
    2 Key Laboratory for Ferrous Metallurgy and Resources Utilization of Ministry of Education, Wuhan University of Science and Technology, Wuhan 430081
  • Received:2013-05-13 Published:2013-12-01 Online:2022-09-07

摘要: 通过热模拟试验,系统分析了定径温度(820~920℃)、应变量(0.18~0.24)和冷却速率(0.2~2.1℃/s)对N80-1无缝套管(Φ139.70~339.72 mm×6.20~22.22 mm)用钢40Mn2V(/%:0.41C、0.22Si、1.65Mn、0.014P、0.005S、0.15V、0.021 Ti、0.008 0N)组织、拉伸强度和冲击功的影响,并建立了数学模型。结果表明,在给定的定径变形温度下,当冷却速率超过某一临界值时,则发生贝氏体转变对低冲击韧性极为不利。40Mn2V钢适合于钢管冷却速率不超过1.1℃/s的钢管规格,当冷却速率低于0.6℃/s时,合适的定径温度为695~870℃,当冷却速率在0.6~1.1℃/s时,定径温度为695~820℃。

Abstract: The influence of sizing deformation temperature (820 ~ 920 °C ) , deformation extent (0. 18 ~ 0. 24) and cooling rate (0. 2 ~2. 1 ℃/s) on structure, tensile strength and impact energy of steel 40Mn2V (/% : 0. 41C, 0. 22Si, 1.65Mn, 0.014P, 0. 005S, 0. 15V, 0.021Ti, 0.008 0N) for N80-1 seamless casing tube (Φ139. 70 ~ 339. 72 mm x 6. 20 ~22. 22 mm) is systematically analyzed by hot simulation test, and a math model is established. Results show that at defined sizing deformation temperature, as cooling rate of steel is higher than a critical value, the bainite transformation occurs in structure led to poor impact toughness of steel; steel 40Mn2V is available for the tube size with cooling rate less than 1. 1 ℃/s, the suitable process parameters are that as cooling rate less than 0. 6 ℃/s, the sizing temperature is 695 ~870℃, and as cooling rate 0. 6 ~ 1. 1 °C/s, the sizing temperature is 695 ~ 820 ℃.