X70管线钢180 t LF深脱硫精炼工艺的优化

邹长东1,赵家七1,周彦召1,耿涛1,丁振涛2   

  1. 江苏省沙钢 1 钢铁研究院 ;2 宏发炼钢厂,张家港 215625
  • 收稿日期:2013-04-24 出版日期:2013-10-01 发布日期:2022-09-22
  • 作者简介:邹长东(1983-),男,博士,(2010年上海大学),研究员,低成本洁净钢冶炼工艺开发

Optimization of 180 t LF Deep Desulphurization Refining Process for Pipeline Steel X70

Zou Changdong1 , Zhao Jiaqi1 ,  ZhouYanzhao1 ,  Geng Tao1 , Ding Zhentao2   

  1. 1 Research Institute of Iron and Steel , 2 Hongfa Steelmaking Works , Jiangsu Shasteel , Zhangjiagang 215625)
  • Received:2013-04-24 Published:2013-10-01 Online:2022-09-22

摘要: X70管线钢的生产流程为KR铁水预脱硫-180 t BOF-LF-RH-板坯连铸工艺。通过优化精炼渣成分和造渣制度,以及根据底吹流量(400-700 L/min)对终点[S]的影响,制定了LF深脱硫工艺。生产试验结果表明,通过控制精炼渣成分(/%)45~55CaO、30~40Al2O3、≤10SiO2、≤10MgO、≤1.5(TFe+MnO),造渣时分两批(首次出钢过程第二批LF到站加入)或多批加入石灰,精炼过程根据炉渣情况适当调渣,LF精炼脱硫期的底吹气体流量为500~700 L/min,可在40 min内将钢液[S]降低到10×10-6以下,满足了管线钢快速深脱硫的需求。

关键词: 180 t LF精炼, X70管线钢, 深脱硫, 底吹气体流量, 工艺优化

Abstract: The production flow sheet for pipeline steel X70 is KR metal pre-desulphuration-180 t BOF-LF-RH-slab CC process. With optimization of refining slag ingredient and slagging operation, and based on effect of bottom gas blowing rate (400-700 L/min) on end [S] , the LF deep desulphurization process has been schemed. Pilot production results show that by controlling refining slag ingredient (/% ) 45-55CaO, 30-40Al2O3, ≤10SiO2 , ≤10Mgo, ≤1.5(TFe + MnO) , with the technology measures including during slagging the lime being added in two separate batch (first in tapping, second at beginning of LF refining) or being added in multi-batch, during LF refining according to slag condition adjusting ingredient of slag, and bottom gas blowing rate 500-700 L/min during LF desulphurization period, the sulphur content in liquid- [S] could be decreased to lower than 10 x 10-6 in 40 min to meet the requirement of quick deep desulphurization for pipeline steel.

Key words: 180 t LF Refining, Pipeline Steel X70, Deep Desulphurization, Bottom Gas Blowing Rate, Process Optimization