ISSN:1003-8620

CN:42-1243/TF

主管:中信泰富特钢集团股份有限公司

主办:大冶特殊钢有限公司

特殊钢 ›› 2023, Vol. 44 ›› Issue (6): 12-18.DOI: 10.20057/j.1003-8620.2023-00068

• 产品研发 • 上一篇    下一篇

锻钢冷轧工作辊冶金质量剖析与电渣工艺改进

霍振全1, 杨立锋2   

  1. 1 邢台德龙机械轧辊有限公司技术质量部,邢台 054000;2 邢台技师学院基础部,邢台 054000
  • 出版日期:2023-12-01 发布日期:2023-11-21
  • 作者简介:霍振全(1971―),男,本科,高级工程师;E-mail: 2791085404@qq.com

Analysis of Metallurgical Quality of Forged Steel Cold Rolling Work Roll and Improvement of ESR Process

Huo Zhenquan1, Yang Lifeng2   

  1. 1 Technical Quality Department , Xingtai Delong Machinery Roll Co., Ltd., Xingtai 054000 , China;2 Basic Department , Xingtai Technician College , Xingtai 054000 , China
  • Published:2023-12-01 Online:2023-11-21

摘要: 对锻钢冷轧工作辊的冶金质量缺陷的夹杂物超标、碳化物偏析及表面随机缺陷(DRS)三个典型问题进行深入研究和剖析。通过采用改进电渣密封罩和电渣气氛保护,氧浓度在0.001 0%左右,夹杂物超标率降低4%~5%;通过电渣水冷强化对水质和进水温度的改善,控制进水温度15~35 ℃,进回水水温差4~5 ℃,液析碳化物偏析合格率接近100%;通过电渣锭细长化改变电渣锭的规格,表面随机缺陷DRS合格率由85%提升至92%,冷轧工作辊冶金质量得到有效改善。

关键词: 冷轧工作辊冶金质量, 电渣气氛保护改进, 电渣水冷强化改善, 电渣锭细长化改变

Abstract: The three typical problems of metallurgical quality defects of forged steel cold rolling work rolls, including inclusion exceeding the standard, carbide segregation and surface random defects (DRS), were thoroughly studied and analyzed. By adopting the improved ESR sealing cover and atmosphere protection, the oxygen concentration was around 0.001 0%, and the inclusion exceeding rate was reduced by 4%-5%; Through the improvement of water quality and inlet water temperature by water cooling strengthening of electric slag, achieving a control range of inlet temperature of 15-35 ℃, inlet and outlet water temperature difference of 4-5 ℃, and a qualified rate of liquid carbide segregation was close to 100%; The specification of the ESR ingot was changed by the elongation of the ESR ingot, the DRS qualification rate for surface random defects has increased from 85% to 92%, and the metallurgical quality of the cold rolling roll is effectively improved.

Key words: Metallurgical Quality of Cold Rolling Work Roll, Improvement of ESR Atmosphere Protection, Perfected of ESR Water Cooling Strengthening, Change of ESR Ingot Elongation