杨万良, 李京社, 杨宏博, et al. Numerical Simulation on Optimization of Shrinkage Cavity Defect of Steel SCM822H 3 t Ingot[J]. Special Steel, 2013, 34(5): 16-19.
杨万良, 李京社, 杨宏博, et al. Numerical Simulation on Optimization of Shrinkage Cavity Defect of Steel SCM822H 3 t Ingot[J]. Special Steel, 2013, 34(5): 16-19.DOI:
Based on the measured value of ingot surface temperature in ingot stripping at situ
with using ProCAST software the calculation model for filling and solidifying process of 3 t ingot (body height 1675 mm
hot top inclined angle 65. 3°
height of liquid surface in hot top 290 mm) of steel SCM822H (/% : 0.20C
0.80Mn
0.25Si
0.013P
0.006S
1.14Cr
0.39Mo
0.01V
0.036Al
0.0002B) has been established. With calculation by the model the relation between hot top inclined angle
ingot body height-width ratio and body cut-off volume ratio caused by shrinkage cavity is gotten to get the optimized ingot parameters i. e. body height-width ratio 1846/630 and hot top inclined angle 90°. According to optimized ingot mould parameters the simulation results show that with using the new ingot mould the ingot body cut-off volume ratio decreases from original 13. 5% to 0