The austenite stainless steel 204Cu (/% : 0.125-0.131C
0.32-0.34Si
8.51-8.73Mn
0.002-0.006S
0.035-0.047P
16.40-16.64Cr
2.53-2.72Ni
2.33-2.38Cu
0.257-0.271N
0-0.064Ce) is melted by a 10 kg vacuum induction furnace
forged to 25 mm x 25 mm square billet
and solid-solution-treated at 1150 ℃ for 2 h
water cooling. The effect of 0-0.064% Ce on corrosion-resisting properties of stainless steel 204Cu in 3.5% NaCl solution at 25 ℃ has been studied by using weight method
electrochemical polarization curves and AC impedance techniques. Results show that adding definite earth element Ce in stainless steel 204Cu
the anod polarization voltage value shifts positively
the corrosion current density decreases and the polarization resistance increases
that can obviously increase its corrosion-resisting properties
as adding 0.029% Ce the stainless steel 204Cu has optimizing corrosion-resisting properties.