石灰消耗从46.7 kg/t降低到30.2 kg/t;轻烧镁球消耗从13.3 kg/t降低到8.7 kg/t;氧气消耗为47.7 m
3
/t;钢铁料消耗从1075.3 kg/t降低到1072.1 kg/t
实现安全、低成本少渣冶炼。
Abstract
The lesser slag steelmaking process of 150 t BOF by using green dolomite to replace partial lime and magnesia granule is carried out at Shiheng Special Steel
and the safety of heel slag remaining operation is improved by using optimizing " slag splashing + slag adjusting" process; with reasonable slag forming schedule
blowing scheme
adding suitable slag foaming agents and controlling slagging point
the dephosphorization rate of liquid is about 60% and the slagging rate is about 50% to effectively ensure the BOF steelmaking end-point
and the each index gets optimization i. e. the consumption of lime decreases to 30. 2 kg/t from 46. 7 kg/t
the consumption of light burned magnesia granule decreases to 8. 7 kg/t from 13. 3 kg/t
the consumption of oxygen is 47. 7 m
3
/t and the iron and steel material charging decreases to 1072. 1 kg/t from 1075.3 kg/t to realize steelmaking with safe