王百顺, 冯文甫, 郭键, et al. Production Practice of Decreasing Total Oxygen Content in Steel 0Crl3 Steelmaking by Dephosphorized Metal -60 t AOD-LF-150mm x150mm CCM[J]. Special Steel, 2018, 39(1): 34-36.
王百顺, 冯文甫, 郭键, et al. Production Practice of Decreasing Total Oxygen Content in Steel 0Crl3 Steelmaking by Dephosphorized Metal -60 t AOD-LF-150mm x150mm CCM[J]. Special Steel, 2018, 39(1): 34-36.DOI:
With the thermal compensation technology including using CO secondary burning
3.5% ~5.0% Si high carbon ferrochromium and alloys baking
the reduced product SiO
decreases by 800 kg to increase the deoxidation ability of silicon; with controlling AOD slag basicity 2.3~2.4 and carried out secondary reduction in AOD refining
and adding 5 kg/t active lime in LF refining process
the efficiency of deoxidation and desulphurization increases by more than 30% ; and with ( CaO)/( SiO
2
)= 2.2 of CaO-SiO
2
-MgO slag series controlling adding amount of fluorite amounting to 13%~17% of the total lime to get better slag viscosity and be available to slagging and absorbing inclusions
the total oxygen content in Φ5.5 mm wire rod decreases to
30 x 10
-6
~ 40 x 10
-6
from 60 x 10
-6
~ 90 x 10
-6
before optimization and the S content decreases to 0.003% ~0.007% from original 0.005% ~ 0.010% .