陆江帆, 张立红, 桑卫钧. Effect of Solid-Solution-Treated Temperature on Grain Growth Tendency of Φ63mmx10mm Cold-Rolled Tube of Alloy NS3105[J]. Special Steel, 2018, 39(2): 47-50.
陆江帆, 张立红, 桑卫钧. Effect of Solid-Solution-Treated Temperature on Grain Growth Tendency of Φ63mmx10mm Cold-Rolled Tube of Alloy NS3105[J]. Special Steel, 2018, 39(2): 47-50.DOI:
0.0100N) is melted by 12t vacuum induction furnace and electro-slag remelting to 3t ingot with shielding atmosphere
forged breaking-down to Φ236 mm bloom
hot extrusion to Φ95mmx16mm pierced shell
then cold-rolled to Φ63mmx10mm tube. Effect of the solid-solution treatment of cold-rolled tube at 800〜1140°C for 5~15min on structure of steel has been studied. Results show that as the alloy NS3150 hot-worked tube cold-rolled with 60% deformation
the original equiaxed crystal structure of alloy occur large deformation
the deformed grains in cold-rolled tube start to recover-recrystallize at 800°C and the recrystallization is completed basically at 950°C;with increasing temperature and heating time the recrystallized grains of cold-rolled tube grow continuously
and the grains grow inhomogeneously at 950〜1080°C and the mix-grain and coarse-fine grain structure occur; at 1080~1120°C the grains grow homogeneously; and at more than 1120°C the grains of cold-rolled tube grow obviously and the structure is coarser. The optimum solid-solution treated temperature for cold-rolled tube of alloy NS3105 is 1080~1120°C.