吴明, 杨芳, 吕鸣. Effect of Ratio of Lime to Magnesium Powder in Combined Blowing Process on Desulfurization results of Hot Metal[J]. Special Steel, 2018, 39(5): 18-20.
吴明, 杨芳, 吕鸣. Effect of Ratio of Lime to Magnesium Powder in Combined Blowing Process on Desulfurization results of Hot Metal[J]. Special Steel, 2018, 39(5): 18-20.DOI:
Principle and feature of combined blowing process of lime to magnesium for desulfurization of hot metal are briefly introduced
and the effect of ratio of lime to magnesium powder 2. 0 ~ 3. 5 : 1
3.5 ~ 5. 0 : 1 and 5.0 ~ 6.5:1 on end sulfur in metal
resulphurization rate
iron loss and temperature drop in blowing process
desulphurization time and 120 t BOF steelmaking results are commercial-tested. It is obtained that with using the ratio of lime to magnesium powder 3. 5 ~5. 0 : 1
the resulphurization amount is less than 0.003 5%
the iron loss is less than 26 kg/t
temperature drop is less than 18 ℃ and the yield of steel liquid is more than 87%