摘要: 鄂钢股份有限公司采用70tConsteel超高功率电弧炉70t钢包精炼炉4流150mm×150mm方坯连铸连轧工艺生产耐热螺杆高强度标准件用钢B7(40CrMnMo)。电弧炉炉料为30%生铁+70%优质废钢,废钢预热温度≥600℃。生产结果表明,该钢成品化学成分可稳定控制(%):0.39~0.42C,0.86~0.91Mn,0.22~0.31Si,0.013~0.018P,0.005~0.013S,0.85~0.94Cr,0.16~0.18Mo,0.019~0.028Als,偏析与疏松级别为0.5~1.0,夹杂物0.5~2.0级,Φ18~Φ50mm钢材晶粒度8.5~9级,满足耐热螺杆标准件的使用要求。