锻造变形方式对叶片钢1Cr12Ni2Mo2VN横向冲击韧性的影响

陈 列1,曹小军1,佐 辉1,钱才让1,刘雅政2,李俊儒2,甄建才1,晁智勇1   

  1. 1. 西宁特殊钢股份有限公司,西宁 810005 ;
    2. 北京科技大学材料科学与工程学院,北京 100083;
  • 收稿日期:2014-10-25 出版日期:2015-04-01 发布日期:2022-08-23
  • 作者简介:陈列(1968-),男,博士(北京科技大学),1990年北京科技大学(本科)毕业,特殊钢的工艺技术、质量及新产品研发 工作。
  • 基金资助:
    国家(863计划)课题资助项目(2012AA03A502)

Effect of Forging Method on Horizontal Impact Toughness of Blade Steel lCrl2Ni2Mo2VN

Chen Lie1 , Cao Xiaqjun1 , Zuo Hui1 , Qian Cairang1 , Liu Yazheng2 , Li Junru2 , Zhen Jiancai1 ,  Chao Zhiyong1   

  1. 1. Xining Special Steel Co Ltd, Xining 810005 ;
    2. School of Materials Science and Engineering,University of Science and Technology, Beijing 100083;
  • Received:2014-10-25 Published:2015-04-01 Online:2022-08-23

摘要: 分析了常规锻造-拔长,镦粗-拔长,镦粗-拔长-镦粗-拔长,镦粗-换向拔长 4种锻造方式对叶片钢1Cr12Ni2Mo2VN(%:0.10C,0.17Si,0.74Mn,0.014P,0.002S,11.8Cr,2.43Ni,1.65Mo,0.32V,0.0352N)2.5t电渣锭锻造成Φ220 mm棒材横向冲击韧性的影响。结果表明,单道次大压下量的镦拔锻造及镦拔次数的增加可显著提高叶片钢的横向冲击韧性,2镦2拔后的棒材经1050℃1h油冷,660℃2h空冷后的横向冲击功为141 J,横纵向冲击值比可达90%以上,组织均匀,晶粒细化。

关键词: 叶片钢lCr12Ni2Mo2VN, 镦拔锻造, 横向冲击韧性

Abstract: The effect of four forging methods i. e. conventional forging-stretching, upsetting-stretching, upsetting-stretching-upsetting- stretching and upsetting-changing direction stretching on horizontal impact toughness of Φ200 mm bar products forged from 2.5 t ESR ingot of blade steel 1Cr12Ni2Mo2VN (/% : 0.10C, 0.17Si, 0.74Mn, 0.014P, 0.002S, 11.8Cr, 2.43Ni, 1.65Mo, 0.32V, 0.0352N) has been analyzed. The results show that the upsetting-stretching forging with single pass large reduction and increasing upsetting-stretching forging times are available to obviously increase the horizontal impact toughness of blade steel ; with upsetting-stretching-upsetting-stretching process the horizontal impact energy of bar product heated at 1050 ℃for 1 h, oil cooling and at 660 °C for 2 h, air cooling is 141 J, the ratio of horizontal and longitudinal impact energy is more than 90% , and steel structure is uniformity with finer grains.

Key words: Blade Steel 1Cr12Ni2Mo2VN, Upsetting-Stretching Forging, Horizontal Impact Toughness