谭建兴, 武鹏, 刘睿智, et al. Process Practice of Titanium Stabilizing Austenite Stainless Steel 321 Produced by EAF-AOD-LF-Slab Casting[J]. Special Steel, 2018, 39(3): 28-30.
谭建兴, 武鹏, 刘睿智, et al. Process Practice of Titanium Stabilizing Austenite Stainless Steel 321 Produced by EAF-AOD-LF-Slab Casting[J]. Special Steel, 2018, 39(3): 28-30.DOI:
The production flowsheet of titanium stabilizing austenite stainless steel 321 (/% : 0. 04 ~0
08C
0.40 ~ 0.70Si
0. 80~1.50Mn
≤ 0.035P
≤ 0.005S
17. 0 ~ 18. 0Cr
9.0~9.5Ni
0
20~0.40Ti
≤ 0.0200N) is 90t EAF45 t AOD-LF-180 mm x 1 238 mm slab casting. The "floater" in liquid of steel in mold occurs and the nozzle blocking produces in casting process. Based on analysis on TiN precipitation rule it is obtained that in order to decrease of TiN precipitation in liquid it should be controlled [N
]
≤ 0.015 0%
[Ti
]
≤0.25% and temperature of liquid in tundish 〜 1 500 °C. With process measures including using extra-pure Ar stirring in whole AOD process
controlling ladle slag t
hickness 150 mm
[O
]
15 x 10
-6
~20 x 10
-6
and [N
]
~ 110 x 10
-6
and using shielding slag with basicity 0. 75 and viscosity 0. 165 pa ·s at 1 300 ℃
the yield of Ti increases from original 40% to 52%
the N content in finished liquid decreases from 0.014 0% to 0.010 5%
the inner diameter of nozzle at finished casting increases from original 42 mm to 50 mm
and the defect of rolled products decreases from original 3. 5% to 1. 2% .