An Analysis on Break of Separating Ring for Horizontal Concasting and Improved Measures
|更新时间:2026-01-21
|
An Analysis on Break of Separating Ring for Horizontal Concasting and Improved Measures
Special SteelVol. 26, Issue 4, Pages: 46-48(2005)
作者机构:
湖南衡阳钢管(集团)有限公司,衡阳,421001
作者简介:
基金信息:
DOI:
CLC:
Received:26 December 2004,
Online First:17 May 2023,
Published:17 May 2005
稿件说明:
移动端阅览
田汉蒲, 徐景峰, 崔泽南, et al. An Analysis on Break of Separating Ring for Horizontal Concasting and Improved Measures[J]. Special Steel, 2005, 26(4): 46-48.
DOI:
田汉蒲, 徐景峰, 崔泽南, et al. An Analysis on Break of Separating Ring for Horizontal Concasting and Improved Measures[J]. Special Steel, 2005, 26(4): 46-48.DOI:
An Analysis on Break of Separating Ring for Horizontal Concasting and Improved Measures
The chemical composition of separating ring and concasting process have been improved by analysis on break of separating ring for horizontal concasting φ130 mm billet for tube and test of effect of separating ring composition on properties. The results showed that with using B-Sis N
4+
30% BN separating ring
manufactured size precision of separating ring up to 0.1 mm
controlling [N
]
no more than 60×10
-6
[O
]
no more than 30×10
-6
and reverse bush between 3 mm and 5 mm
the break of separating ring was controlled effectively
the average break ratio of separating ring per month de- creased to less than 0.3% from original 8.3%.