Effect of Control Rolling and Aging on Structure and Properties of 570MPa Ultra Low Carbon Bainitic Steel
|更新时间:2026-01-21
|
Effect of Control Rolling and Aging on Structure and Properties of 570MPa Ultra Low Carbon Bainitic Steel
Special SteelVol. 26, Issue 6, Pages: 26-28(2005)
作者机构:
宝山钢铁股份有限公司研究院,上海,201900
作者简介:
基金信息:
DOI:
CLC:
Received:21 June 2005,
Online First:11 April 2023,
Published:11 April 2005
稿件说明:
移动端阅览
张爱文. Effect of Control Rolling and Aging on Structure and Properties of 570MPa Ultra Low Carbon Bainitic Steel[J]. Special Steel, 2005, 26(6): 26-28.
DOI:
张爱文. Effect of Control Rolling and Aging on Structure and Properties of 570MPa Ultra Low Carbon Bainitic Steel[J]. Special Steel, 2005, 26(6): 26-28.DOI:
Effect of Control Rolling and Aging on Structure and Properties of 570MPa Ultra Low Carbon Bainitic Steel
The ulra low carbon bainitic steel ULCB570(0.02C- 1.55Mn-0.62Ni-0.53Cu-0.0035B-0.055V-0.019Ti- 0.028Nb was melted by a 50 kg vacuum induction furnace in laboratory
of which the 25 mm finished plate was rolled from forged 80 mm slab with beginning rolling temperature 1150 ℃
finishing temperature 900 ℃ and air cooling. The continuous cooling transformation curves of deforming austenite was measured by a Thermecmaster-Z thermal simulation machine. The results showed that the structure of steel deformed with cooling rate 0. 1~30 ℃/s was bainite-ferrite + secondary phase (precipitates);the tensile strength on of steel as rolled condition was 595 MPa
impact toughness A
KV
180 J
of which as rolled + 600 ℃ aged condition the tensile strength σ
b
of steel increased to 610 MPa
impact t
oughness A
KV
to 202 J to meet the requirement for properties of 570 MPa steel plate.