A Study on Molten Slag Layer and Slag Film of Mould Flux used in Slab Casting of Stainless Steel 1Crl7
|更新时间:2026-01-21
|
A Study on Molten Slag Layer and Slag Film of Mould Flux used in Slab Casting of Stainless Steel 1Crl7
Special SteelVol. 30, Issue 3, Pages: 16-18(2009)
作者机构:
1. 北京科技大学冶金与生态工程学院,北京,100083
2. 青岛斯多伯格三一冶金材料有限公司,青岛,266300
3. 宝钢研究院不锈钢技术中心,上海,201900
作者简介:
基金信息:
DOI:
CLC:
Received:01 December 2008,
Online First:22 November 2022,
Published:22 November 2009
稿件说明:
移动端阅览
郝占全, 陈伟庆, CarstenLippold, et al. A Study on Molten Slag Layer and Slag Film of Mould Flux used in Slab Casting of Stainless Steel 1Crl7[J]. Special Steel, 2009, 30(3): 16-18.
DOI:
郝占全, 陈伟庆, CarstenLippold, et al. A Study on Molten Slag Layer and Slag Film of Mould Flux used in Slab Casting of Stainless Steel 1Crl7[J]. Special Steel, 2009, 30(3): 16-18.DOI:
A Study on Molten Slag Layer and Slag Film of Mould Flux used in Slab Casting of Stainless Steel 1Crl7
Main ingredients of test mould powder were ( % ) 35. 46CaO
32. 84SiO
2
7. 87Al
2
O
3
3. 04MnO
8. 48Na
2
O
7. 13F
2. 6C. Samples of mould molten slag and slag film during casting of stainless steel !Crl7 were taken to study the change of ingredients and properties of molten slag and performance of slag film. Results showed that at casting for less than 10 min
the Al
2
O
3
and Cr
2
O
3
content in molten slag definitely increased while basicity of molten slag slightly decreased
but for more than 10 min the contents were trending towards stability: as compared to fresh slag the melting temperature and viscosity of molten slag increased of which the change of solidification temperature was minor; the melting t
emperature of molten slag after change ingredient was still in suitable range
although the viscosity of molten slag increased by 0. 08 Pa
s; the slag film consisted of crystal layer and glassy layer
the crystallization ratio of slag film was about 71% and the main phases of film were cuspidite crystals with minor nepheline crystals.