DOI:
尹娜, 景财良, 张炯明, et al. Optimization of Mold Powder for H-Shape Steel Q235B Casting[J]. Special Steel, 2010, 31(2): 40-42. DOI:
针对津西钢铁厂H型钢Q235B(0.14%~0.18%C)铸坯(宽面550 mm
窄面440 mm
腹板90 mm)经常出现纵裂等缺陷
基于原有保护渣(%:29~30SiO2、25~26CaO、10~11Al2O3、3.0~3.5Fe
2
O
3
、15~17C、≤0.5H
O)
通过正交实验和优化设计
开发出一种高性能保护渣(%:37.50SiO
、37.50CaO、6Al
、7CaF
、12Na
O、7石墨、1.5炭黑)。与原保护渣相比
优化渣的半球点温度、粘度和熔化时间分别从1 167℃
0.77 Pa·s和57 s下降至1 092℃
0.27 Pa·s和32.5 s。优化渣应用表明
当拉速由0.98 m/min提高到1.2 m/min时
铸坯质量良好。
To counter the situation of longitudinal crack defect usually occurred on bloom (wide side 550 mm
narrow side 440 mm
waist 90 mm) in H-shape steel Q235B (0. 14% ~0. 18%C) casting at Jinxi Iron and Steel works
based on original mold powder (% : 29~30Si02
25 ~26CaO
10 ~ 11A12O3
3. 0 ~ 3.5Fe
15 ~ 17C
≤0.5H
a high performance mold powder (% : 37. 50Si0
37. 50CaO
6A1
7CaF
12Na
7 graphite
1. 5 carbon black) is developed by orthogonal experimental and optimum design. As compared with original mold powder
the semi-sphere point temperature
viscosity and melting time of improved mold powder decrease respectively to 1 092 ℃
0. 27 Pa • s and 32. 5 s from original 1 167℃
0. 77 Pa • s and 57
s. Application shows that as casting speed increase from 0. 98 m/min to 1. 2 m/min
the bloom has high quality by using the improved mold powder.