Effect of Annealing Temperature on Structure and Mechanical Properties of Hot-rolled 0.14C-5Mn Steel
|更新时间:2026-01-21
|
Effect of Annealing Temperature on Structure and Mechanical Properties of Hot-rolled 0.14C-5Mn Steel
Special SteelVol. 34, Issue 1, Pages: 56-58(2013)
作者机构:
1. 太原钢铁(集团)有限公司技术中心,太原,030003
2. 钢铁研究总院,北京,100081
3. 西部钛业有限责任公司.,西安,710201
作者简介:
基金信息:
DOI:
CLC:
Received:25 July 2012,
Online First:14 September 2022,
Published:14 September 2013
稿件说明:
移动端阅览
石发才, 王存宇, 李楠, et al. Effect of Annealing Temperature on Structure and Mechanical Properties of Hot-rolled 0.14C-5Mn Steel[J]. Special Steel, 2013, 34(1): 56-58.
DOI:
石发才, 王存宇, 李楠, et al. Effect of Annealing Temperature on Structure and Mechanical Properties of Hot-rolled 0.14C-5Mn Steel[J]. Special Steel, 2013, 34(1): 56-58.DOI:
Effect of Annealing Temperature on Structure and Mechanical Properties of Hot-rolled 0.14C-5Mn Steel
0. 003 ON) is melted by a 50 kg vacuum induction furnace and roiled to 4 mm pate (finishing temperature 1 000 °C
air cooling). The structure and mediatic properties of 4 mm plate of 0. 14C-5Mn steel annealed at 550 ~ 650 °C for 6h are studied by scanning electron microscope
X-ray diffraction analysis and uniaxial tensile test. Results show that the austenite is produced in annealing process of 0. 14C-5Mn steel (occurring transformation-induced plasticity-TRIP effect)
and with increasing annealing temperature the volume fraction of austenite increases and the elongation and product of tensile strength to elongation increase obviously. With annealing at 650 °C for 6 li the austenite fraction in steel is up to 30. 11%
the tensile strength of steel is 945 MPa and the product of tensile strength to elongation is 37. 3 GPa%.