Evolution of Inclusions in Stainless Steel 304 during Dephosphorized Hot Metal-110 t AOD-LF-CC-Hot Rolling Process
|更新时间:2026-01-21
|
Evolution of Inclusions in Stainless Steel 304 during Dephosphorized Hot Metal-110 t AOD-LF-CC-Hot Rolling Process
Special SteelVol. 34, Issue 1, Pages: 41-44(2013)
作者机构:
1. 北京科技大学钢铁冶金新技术国家重点实验室,北京,100083
2. 酒泉钢铁集团公司,嘉峪关,735100
作者简介:
基金信息:
DOI:
CLC:
Received:20 June 2012,
Online First:14 September 2022,
Published:14 September 2013
稿件说明:
移动端阅览
陈超, 侯海滨, 成国光, et al. Evolution of Inclusions in Stainless Steel 304 during Dephosphorized Hot Metal-110 t AOD-LF-CC-Hot Rolling Process[J]. Special Steel, 2013, 34(1): 41-44.
DOI:
陈超, 侯海滨, 成国光, et al. Evolution of Inclusions in Stainless Steel 304 during Dephosphorized Hot Metal-110 t AOD-LF-CC-Hot Rolling Process[J]. Special Steel, 2013, 34(1): 41-44.DOI:
Evolution of Inclusions in Stainless Steel 304 during Dephosphorized Hot Metal-110 t AOD-LF-CC-Hot Rolling Process
通过扫描电镜、能谱仪和电解分析研究了在110 t AOD-LF-中间包-160 mm板坯-连铸-热轧板卷生产过程304不锈钢(/%:0.03~0.04C、0.39~0.41Si、1.20~1.23Mn、0.014~0.016P、0.001~0.002S、7.95~8.00Ni、18.06~18.20Cr、0.003~0.004Al、0~0.002Ti)中夹杂物类型、形貌和成分。结果表明
morphology and ingredient of inclusions in stainless steel 304 (/%: 0. 03 ~0. 04C
0. 39 ~0. 41 Si
L20~1.23Mn
0. 014 ~0. 016P
0.001 ~0.002S
7.95 〜8.00Ni
18. 06 ~ 18. 20Cr
0.003 ~ 0. 004Al
0 〜0.002Ti) during 110 t AOD-LF-tundish-160 mm slab casting-hot rolling strip coil process have been studied by SEM
energy dispersive X-ray spectrometer and analysis by electrolysis. Results show that the 5 ~ 10 μm spheroidal SiO
2
-CaO-MgO-Al
2
0
3
type inclusions occur in each steelmaking process
while the 20 μm MnO-Cr
2
O
3
inclusions form in tapping proc
ess of AOD
part of which is removed in LF refining process
and they less occur in liquid in tundish and in normal casting slab
but the MnO-Cr
2
O
3
inclusions easily occur in two heats sequence-casting slab
the size of MnO-Cr
2
O
3
inclusion in hot-rolled strip coil is≤5μm. Electrolytic analysis results show that the inclusion amount in two heats sequence-casting slab (4. 65 mg/ 10 kg) increases by 51% as compared with that in normal casting slab (3. 08 mg/10 kg).