Influence of Sizing and Cooling Process on Structure and Mechanical Properties of N80-1 Seamless Casing Tube of Steel 40Mn2V
|更新时间:2026-01-21
|
Influence of Sizing and Cooling Process on Structure and Mechanical Properties of N80-1 Seamless Casing Tube of Steel 40Mn2V
Special SteelVol. 34, Issue 6, Pages: 45-48(2013)
作者机构:
1. 衡阳华菱钢管(集团)有限公司技术中心,衡阳,421001
2. 武汉科技大学钢铁冶金及资源利用省部共建教育部重点实验室,武汉,430081
作者简介:
基金信息:
DOI:
CLC:
Received:13 May 2013,
Online First:07 September 2022,
Published:07 September 2013
稿件说明:
移动端阅览
吴乐胜, 方剑, 李明新, et al. Influence of Sizing and Cooling Process on Structure and Mechanical Properties of N80-1 Seamless Casing Tube of Steel 40Mn2V[J]. Special Steel, 2013, 34(6): 45-48.
DOI:
吴乐胜, 方剑, 李明新, et al. Influence of Sizing and Cooling Process on Structure and Mechanical Properties of N80-1 Seamless Casing Tube of Steel 40Mn2V[J]. Special Steel, 2013, 34(6): 45-48.DOI:
Influence of Sizing and Cooling Process on Structure and Mechanical Properties of N80-1 Seamless Casing Tube of Steel 40Mn2V
The influence of sizing deformation temperature (820 ~ 920 °C )
deformation extent (0. 18 ~ 0. 24) and cooling rate (0. 2 ~2. 1 ℃/s) on structure
tensile strength and impact energy of steel 40Mn2V (/% : 0. 41C
0. 22Si
1.65Mn
0.014P
0. 005S
0. 15V
0.021Ti
0.008 0N) for N80-1 seamless casing tube (Φ139. 70 ~ 339. 72 mm x 6. 20 ~22. 22 mm) is systematically analyzed by hot simulation test
and a math model is established. Results show that at defined sizing deformation temperature
as cooling rate of steel is higher than a critical value
the bainite transformation occurs in structure led to poor impact toughness of steel; steel 40Mn2V is available for the tube size with cooling rate less than 1. 1 ℃/s
the suitable process parameters are that as cooling rate less than 0. 6 ℃/s