Process Practice for Production of Non-Quenched and Tempered Steel by 100 t EAF-LF-VD-CC Flow Sheet
|更新时间:2026-01-21
|
Process Practice for Production of Non-Quenched and Tempered Steel by 100 t EAF-LF-VD-CC Flow Sheet
Special SteelVol. 34, Issue 4, Pages: 46-48(2013)
作者机构:
苏钢集团技术中心,苏州,215151
作者简介:
基金信息:
DOI:
CLC:
Received:03 March 2013,
Online First:11 September 2022,
Published:11 September 2013
稿件说明:
移动端阅览
黄周华, 左立杰, 颜丽华. Process Practice for Production of Non-Quenched and Tempered Steel by 100 t EAF-LF-VD-CC Flow Sheet[J]. Special Steel, 2013, 34(4): 46-48.
DOI:
黄周华, 左立杰, 颜丽华. Process Practice for Production of Non-Quenched and Tempered Steel by 100 t EAF-LF-VD-CC Flow Sheet[J]. Special Steel, 2013, 34(4): 46-48.DOI:
Process Practice for Production of Non-Quenched and Tempered Steel by 100 t EAF-LF-VD-CC Flow Sheet
非调质钢S38MnSiV(/%:0.41~0.45C、0.55~0.70Si、1.40~1.55Mn、≤0.025P、≤0.025S、0.10~0.20Cr、0.11~0.15V、0.012 0~0.020 0N)的生产流程为40%铁水+废钢-100 t EAF-LF-VD-160 mm×160 mm~260mm×340 mm CC工艺。通过控制电弧炉出钢终点[C
]
0.15%~0.30%
出钢[P
]
≤0.012%
出钢温度1 640~1 680℃
高碱度渣精炼
控制钢液铝含量
VD后喂氮化锰线控制钢液中氮含量等工艺措施
8炉生产结果表明
钢中氧含量-[O
]
5×10
-6
~11×10
-6
[H
]
1.2×10
-6
~1.5×10
-6
[N
]
135×10
-6
~180×10
-6
260 mm×340 mm铸坯热孔成Φ140 mm棒材经880℃ 120 min正火风冷
580℃ 240 min回火空冷后的抗拉强度Rm为870~925 MPa
屈服强度Rel为560~605 MPa
其冶金质量满足标准要求。
Abstract
The production flow sheet of non-quenched and tempered steel S38MnSiV (/%: 0.41 ~0.45C
0.55 ~ 0.70Si
1.40~1.55Mn
≤0.025P
≤0.025S
0.10 ~ 0.20Cr
0.11 ~ 0.15V
0.012 0 ~ 0.020 ON) is 40% hot metal + scrap-100 t EAF-LF-VD-160 mm x 160 mm ~260 mm x 340 mm CC process. With controlling arc furnace tap end [C
]
0.15% ~ 0.30%
tapping [P
]
≤0. 012%
tapping temperature 1 640 ~ 1 680 °C
refining by high basicity slag
controlling aluminum content in liquid
after VD feeding manganese-nitride wire to control nitrogen content in liquid etc. process measure
the 8 heat steelmaking results show that oxygen content in steel- [O
]
x 10
-6
-11 x
10
-6
[H
]
1.2 x 10
-6
1. 5 x 10
-6
and [N
]
135 x 10
-6
- 180 x 10
-6
for the Φ140 mm round bar products rolled from 260 mm x 340 mm casting bloom with normalizing at 880℃ for 120 min
airflow cooling and tempered at 580℃ for 240 min air cooling
the tensile strength Rm is 870 ~925 MPa and the yield strength Re
]
is 560 - 605 MPa
its metallurgy quality all meets the requirement of standard.