Practice of Production on Cutting-down Consumption of Electric Power for 150 t LF Refining
|更新时间:2026-01-21
|
Practice of Production on Cutting-down Consumption of Electric Power for 150 t LF Refining
Special SteelVol. 35, Issue 1, Pages: 33-35(2014)
作者机构:
安阳钢铁集团股份有限公司技术中心,安阳,455004
作者简介:
基金信息:
DOI:
CLC:
Received:26 August 2013,
Online First:05 September 2022,
Published:05 September 2014
稿件说明:
移动端阅览
裴凤娟, 黄重, 向华, et al. Practice of Production on Cutting-down Consumption of Electric Power for 150 t LF Refining[J]. Special Steel, 2014, 35(1): 33-35.
DOI:
裴凤娟, 黄重, 向华, et al. Practice of Production on Cutting-down Consumption of Electric Power for 150 t LF Refining[J]. Special Steel, 2014, 35(1): 33-35.DOI:
Practice of Production on Cutting-down Consumption of Electric Power for 150 t LF Refining
With the process measures including increasing temperature of liquid in BOF tapping ( steel Q235A/Q35B 1 660 ~ 1 670 °C
steel Q345A/Q345B 1 665 ~ 1 675℃
end [C]≥O. 06%
end [P]≤0.025% )
intensifying ladle turnover administration
reducing down slag amount
adding modifier or desulphurizing agent for slagging and desulphurization in advance and accurately calculating alloys addition during tapping
and controlling ladle bottom argon blowing rate to protect reoxidation of liquid and slag entrapment
the average power on time for refining steel Q235B and steel Q345B in 150 t LF decreases respectively from 8. 10 min and 9. 39 min to 2. 60 min and 3. 13 min
the average electric power consumption reduces respectively from 17. 33 kWh/t and 20. 09 kWh/t to 5. 55 kWh/t and 6. 69 kWh/t
and the average LF refining time decreases respectively from 40 min and 42 min to 20. 1 min and 22. 4 min
all refining indexes are all meet the requirement with getting better economic performance.