Effect of Stress-Relieving Annealing Treatment on Mechanical Properties of 0.12 mm Cold-Rolled Strip of Stainless Steel 301
|更新时间:2026-01-21
|
Effect of Stress-Relieving Annealing Treatment on Mechanical Properties of 0.12 mm Cold-Rolled Strip of Stainless Steel 301
Special SteelVol. 35, Issue 1, Pages: 68-70(2014)
作者机构:
安泰科技股份有限公司北京空港新材分公司,北京,101318
作者简介:
基金信息:
DOI:
CLC:
Received:19 August 2013,
Online First:06 September 2022,
Published:06 September 2014
稿件说明:
移动端阅览
秦红霞. Effect of Stress-Relieving Annealing Treatment on Mechanical Properties of 0.12 mm Cold-Rolled Strip of Stainless Steel 301[J]. Special Steel, 2014, 35(1): 68-70.
DOI:
秦红霞. Effect of Stress-Relieving Annealing Treatment on Mechanical Properties of 0.12 mm Cold-Rolled Strip of Stainless Steel 301[J]. Special Steel, 2014, 35(1): 68-70.DOI:
Effect of Stress-Relieving Annealing Treatment on Mechanical Properties of 0.12 mm Cold-Rolled Strip of Stainless Steel 301
A test for the effect of stress-relieving annealing with unit stress 20 MPa and annealing speed 8. 0 ~ 15. 0 m/min at 250 ~400 Y on mechanical properties of 0. 12 mm strip cold-rolled from 1. 2 mm hot-rolled plate of stainless steel SUS301 (/% : 0. 13C
0. 35Si
1.63Mn
0. 033P
0. 002S
16. 54Cr
6. 27Ni
0. 051N) has been carried out by continuous stress-relieving annealing furnace. Results show that before stress-relieving treatment the HV value
tensile
yield strength and elongation of 0. 12 mm cold-rolled strip of steel 301 are respectively 498
1 623 MPa
1 498 MPa and 6.9% ; with raising annealing temperature
the strength and hardness of cold-rolled sheet of steel 301 increase while the elongation of steel decreases; at definite temperature with increasing annealing rate
the elongation of cold-rolled sheet of steel increases. As annealing at 400 °C with 8. 0 ~ 12. 5 m/min
owing to formation of martensite phase and dislocation migration the hardness HV value of cold-rolled sheet is up to N 525
and the tensile and yield strength are respectively 1 771.7 ~ 1790.0 MPa and 1 566.7 〜1 623. 3 MPa.