Effect of Continuous Annealing Temperature on Structure Texture and Mechanical Properties 390 MPa IF Steel
|更新时间:2026-01-21
|
Effect of Continuous Annealing Temperature on Structure Texture and Mechanical Properties 390 MPa IF Steel
Special SteelVol. 35, Issue 3, Pages: 53-55(2014)
作者机构:
1. 首钢冷轧薄板有限公司,北京,101304
2. 北京科技大学冶金工程研究院,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:08 December 2013,
Online First:01 September 2022,
Published:01 September 2014
稿件说明:
移动端阅览
程晓杰, 李振, 蔡阿云, et al. Effect of Continuous Annealing Temperature on Structure Texture and Mechanical Properties 390 MPa IF Steel[J]. Special Steel, 2014, 35(3): 53-55.
DOI:
程晓杰, 李振, 蔡阿云, et al. Effect of Continuous Annealing Temperature on Structure Texture and Mechanical Properties 390 MPa IF Steel[J]. Special Steel, 2014, 35(3): 53-55.DOI:
Effect of Continuous Annealing Temperature on Structure Texture and Mechanical Properties 390 MPa IF Steel
Test 0. 8 mm cold rolled sheet of 390 MPa IF steel (/%: 0. 005C
0.04Si
0. 35Mn
0. 095P
0. 005S
0. 030Nb
0. 016Ti
0. 036Alt) is cold rolled by 4 mm hot rolled plate. The effect of continuous annealing temperature 780 ~ 820 °C on structure
texture and mechanical properties of the IF steel has been studied. Results show that as continuous annealing temperature increases from 780 ℃ to 820 ℃
the yield and tensile strength of the IF steel decrease respectively from 282 MPa and 432 MPa to 249 MPa and 405 MPa
and the elongation A
50
and plastic strain ratio r
m
increase respectively from 37. 2% and 1.45 to 41. 7% and 1. 84
it has better deep drawing property while with increasing annealing temperature the plane an
isotropic index △r increases from 0. 44 to 0. 65
grain size of ferrite increases, and structure homogeneity becomes poor
and deformation texture {112}
<
110 > is weaker
favorable texture {111}
<
110 > is enhanced
texture {001}
<
110> weakens
comprehensively considering
the suitable annealing temperature is about 820 ℃.