含钛低碳钢(/%:0.05~0.10C、0.70~0.95Si、1.45~1.65Mn、≤0.025P、≤0.025S、0.10~0.20Ti)的生产流程为高炉铁水-35 t LD-LF-150 mm×150 mm连铸工艺。用少量铝脱氧的含钛低碳钢
由于LF精炼渣(/%:55~59CaO、21.9~26.5SiO
2
、9.4~14.3Al
2
O
3
)中Al
2
O
3
含量较高
使LF精炼过程中钢水铝含量增加和20 t中间包水口结瘤
影响连铸顺行。在热力学计算的基础上
优化了冶炼工艺
转炉出钢不加铝锰铁
使用低铝硅铁代替普通硅铁
精炼渣不加高铝矾土
优化精炼渣成分(/%:56.1~65.6CaO、19.3~27.2SiO
2
、5.1~9.1Al
2
O
3
)
钢水中Al含量由0.007%~0.018%降至0.001%~0.009%
有效减少中间包水口结瘤的发生。连浇炉数由原来的3~6炉提高到9~16炉。
Abstract
The production flow sheet for titanium-containing low carbon steel (/% : 0.05-0.10C
0.70-0.95Si
1.45-1.65Mn
≤0.025P
≤0.025S
0.10-0.20Ti) is BF hot metal-35 t LD-LF-150 mm x 150 mm casting process. For titanium-containing low carbon steel deoxidizing by minor aluminium due to higher A1
2
O
3
content in LF refining slag (/% : 55 ~59CaO
21.9-26.5SiO
2
9.4-14.3A1
2
O
3
)
during LF process the aluminium content in liquid increases and the 20 t tundish nozzle blocking easily occurs to effect casting smooth-going. Based on thermodynamics calculation
the steelmaking process is optimum including in BOF tapping non-adding manganese-aluminium iron and using low aluminium
silicon iron to replace common silicon iron
non-adding high alumina in refining slag and optimizing refining slag ingredient (/% : 56.1-65.6CaO
19.3-27.2SiO
2
5.1-9.1 Al
2
O
3
)
the Al content in liquid decreases from original 0.007%-0.018% to 0.001%-0.009%
it is available to decrease the occurrence of nozzle blocking. The continuous-continuous casting heats increase from original 3 ~6 heats to 9-16 Heats.