Effect of 150 mm x 150 mm Casting Billet Stacking Slow Cooling Process on Carbon Segregation of High Carbon Steel
|更新时间:2026-01-21
|
Effect of 150 mm x 150 mm Casting Billet Stacking Slow Cooling Process on Carbon Segregation of High Carbon Steel
Special SteelVol. 35, Issue 3, Pages: 39-41(2014)
作者机构:
1. 北京科技大学冶金与生态工程学院,北京,100083
2. 辛集市澳森钢铁有限公司,辛集,052360
作者简介:
基金信息:
DOI:
CLC:
Online First:29 August 2022,
Published:29 August 2014
稿件说明:
移动端阅览
邢梅峦, 包燕平. Effect of 150 mm x 150 mm Casting Billet Stacking Slow Cooling Process on Carbon Segregation of High Carbon Steel[J]. Special Steel, 2014, 35(3): 39-41.
DOI:
邢梅峦, 包燕平. Effect of 150 mm x 150 mm Casting Billet Stacking Slow Cooling Process on Carbon Segregation of High Carbon Steel[J]. Special Steel, 2014, 35(3): 39-41.DOI:
Effect of 150 mm x 150 mm Casting Billet Stacking Slow Cooling Process on Carbon Segregation of High Carbon Steel
The coil of high carbon steel SWRH82B (0. 81%C) is used for pre-stressed wire strands
and the serious net carbides in steel is important factor of wire fracture during cold drawing process. The effect of 150 mm x 150 mm casting billet stacking slow cooling time (0 ~48 h) of steel on carbon segregation in billet and carbide segregation in φ 12. 5 mm coil is tested. Results show that the deviation of carbon content in billet with direct air cooling is 0. 116%
after stacking slow cooling of billet for 12
24
36 and 48 h
the deviation carbon content in billet respectively decreases to 0. 088%
0. 080%0. 075% and 0. 076%
and the rating of net carbide in coil is also corresponding decreased ; it is available to meet the requirement for cold drawing process by stacking slow cooling for 24 h of steel SWRH82B 150 mm x 150 mm casting billet.