Effect of Carbon Content and Casting Parameters on Heat Flux of Mold for Wide-Thick Slab during Concasting Process
|更新时间:2026-01-21
|
Effect of Carbon Content and Casting Parameters on Heat Flux of Mold for Wide-Thick Slab during Concasting Process
Special SteelVol. 35, Issue 4, Pages: 36-40(2014)
作者机构:
1. 大连理工大学材料科学与工程学院,大连,116024
2. 江苏沙钢集团,张家港,215625
作者简介:
基金信息:
DOI:
CLC:
Received:24 February 2014,
Online First:03 September 2022,
Published:03 September 2014
稿件说明:
移动端阅览
王旭东, 尹少华, 孔令伟, et al. Effect of Carbon Content and Casting Parameters on Heat Flux of Mold for Wide-Thick Slab during Concasting Process[J]. Special Steel, 2014, 35(4): 36-40.
DOI:
王旭东, 尹少华, 孔令伟, et al. Effect of Carbon Content and Casting Parameters on Heat Flux of Mold for Wide-Thick Slab during Concasting Process[J]. Special Steel, 2014, 35(4): 36-40.DOI:
Effect of Carbon Content and Casting Parameters on Heat Flux of Mold for Wide-Thick Slab during Concasting Process
The in-line examination and statistics on casting process for 220 ~ 320 mm x 1 800 ~ 2 700 mm wide-thick slab of 0.07% ~0
18% C steel have been carried out for one year at steel work to study the effect of process parameters including casting rate (0.65 ~ 1. 2 m/min)
liquid superheating extent (13-35 ℃)
mold inlet water temperature (27 -35°C) and mold liquid level (775 -810 mm) on heat flux of mold copper plate during casting process of steel grades containing different C%. Results show that with casting 220 mm slab with increasing casting rate the mold heat flux increases
but as casting rate more than 1. 05 m/min
the heat flux doesn't increase again; for the steel grades with peritectic reaction
with increasing liquid superheating extent the heat flux of wide and narrow face o£ slab increases
but with increasing inlet water temperature the heat flux decreases ; due to the effect of peritectic phase transformation
during casting 0.13% C steel the mold heat flux is lowest.