Analysis and Process Practice on Steelmaking Technology of 100 t Top-Blown Oxygen Converter by Limestone for Slag Making
|更新时间:2026-01-21
|
Analysis and Process Practice on Steelmaking Technology of 100 t Top-Blown Oxygen Converter by Limestone for Slag Making
Special SteelVol. 35, Issue 5, Pages: 34-36(2014)
作者机构:
首秦金属材料有限公司,秦皇岛,066326
作者简介:
基金信息:
DOI:
CLC:
Received:28 April 2014,
Online First:01 September 2022,
Published:01 September 2014
稿件说明:
移动端阅览
秦登平, 杨建平, 危尚好, et al. Analysis and Process Practice on Steelmaking Technology of 100 t Top-Blown Oxygen Converter by Limestone for Slag Making[J]. Special Steel, 2014, 35(5): 34-36.
DOI:
秦登平, 杨建平, 危尚好, et al. Analysis and Process Practice on Steelmaking Technology of 100 t Top-Blown Oxygen Converter by Limestone for Slag Making[J]. Special Steel, 2014, 35(5): 34-36.DOI:
Analysis and Process Practice on Steelmaking Technology of 100 t Top-Blown Oxygen Converter by Limestone for Slag Making
With analysis on the mechanism of early stages slag making by limestone and calculation of heat balance in converter
it is obtained that as controlling limestone consumption 6.0 t/heat
the hot metal consumption must increase by 2.1 t/heat and the scrap consumption shall decrease by 2.5 t/heat
it may insure that the end temperature by limestone steelmaking process is the same by lime steelmaking process. Pilot production results show that with limestone slag making technology the converter steelmaking end basicity (3.3)
end temperature (1662 °C )
end [C] (0.081%)
end [P] (0.016% ) and end percentage of hits (90% ) showing no difference from that with conventional lime slag making technology. But with limestone slag making technology the cost of converter stock decreases by 10. 4 yuan /t steel to get better economic and social benefit.