Effect of Design Parameters of Oxygen Lance Nozzle for 110 t Combined Blown Converter on Metallurgical Quality of Liquid Steel
|更新时间:2026-01-21
|
Effect of Design Parameters of Oxygen Lance Nozzle for 110 t Combined Blown Converter on Metallurgical Quality of Liquid Steel
Special SteelVol. 35, Issue 6, Pages: 47-50(2014)
作者机构:
北京科技大学冶金与生态工程学院,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:05 July 2014,
Online First:20 August 2022,
Published:20 August 2014
稿件说明:
移动端阅览
刘煜, 朱荣, 刘福海. Effect of Design Parameters of Oxygen Lance Nozzle for 110 t Combined Blown Converter on Metallurgical Quality of Liquid Steel[J]. Special Steel, 2014, 35(6): 47-50.
DOI:
刘煜, 朱荣, 刘福海. Effect of Design Parameters of Oxygen Lance Nozzle for 110 t Combined Blown Converter on Metallurgical Quality of Liquid Steel[J]. Special Steel, 2014, 35(6): 47-50.DOI:
Effect of Design Parameters of Oxygen Lance Nozzle for 110 t Combined Blown Converter on Metallurgical Quality of Liquid Steel
Based on established geometric model the three dimensional numerical simulation on the effect of oxygen lance nozzle parameters (angle between nozzle 12° ~ 13°
nozzle number 4
flow rate 22000 ~ 24000 m
3
/h) of top and bottom combined blown converter tapping 110 t liquid steel on jet has been carried out by using software Fluent to get that with nozzle angle 12. 5° 4-nozzle oxygen lance at 1. 1 ~ 1. 4 m lance level the suitable radius and higher jet speed may maintain. The application practice of 93 heats 0. 45 C steel
Q235 and HRB400 steel steelmaking at steel works shows that with 12. 5° nozzle angle and oxygen flow rate 22000 m
3
/h
the average tap to tap time of 110 t liquid is 14. 8 min
the end carbon meets the requirement of melting steel grades
the end [P
]
0. 010% ~ 0.030% and the dephosphorizing rate of liquid ≥96%.