Effect of Ladle Top Slag Modification Treatment on Inclusions in Ultra-Low Carbon Steel in 210 t BOF-RH-Slab CC Flowsheet
|更新时间:2026-01-21
|
Effect of Ladle Top Slag Modification Treatment on Inclusions in Ultra-Low Carbon Steel in 210 t BOF-RH-Slab CC Flowsheet
Special SteelVol. 36, Issue 3, Pages: 38-42(2015)
作者机构:
作者简介:
基金信息:
DOI:
CLC:
Received:20 December 2014,
Online First:17 August 2022,
Published:17 August 2015
稿件说明:
移动端阅览
周业连, 何奇, 邓志银, et al. Effect of Ladle Top Slag Modification Treatment on Inclusions in Ultra-Low Carbon Steel in 210 t BOF-RH-Slab CC Flowsheet[J]. Special Steel, 2015, 36(3): 38-42.
DOI:
周业连, 何奇, 邓志银, et al. Effect of Ladle Top Slag Modification Treatment on Inclusions in Ultra-Low Carbon Steel in 210 t BOF-RH-Slab CC Flowsheet[J]. Special Steel, 2015, 36(3): 38-42.DOI:
Effect of Ladle Top Slag Modification Treatment on Inclusions in Ultra-Low Carbon Steel in 210 t BOF-RH-Slab CC Flowsheet
The amount and distribution of inclusions in casting slab of ultra-low carbon steel ( ≤0. 01% C) processing in 210 t ladle with and without adding modifying agent (/% : 38 ~43Al
20~30Al
2
O
3
27 ~ 31 CaO
≤6SiO
2
≤6MgO) to ladle top slag have been examined and analyzed
and the effect of modifying agent on oxygen equilibrium between steel and slag and inclusions in casting slab is studied by thermodynamic analysis. Results show that the ingredient of refining slag sample for ladle top slag with
out adding modifying agent is (/% ) 25. 55 ~ 39. 68CaO
8. 51 ~15. 14SiO
2
6. 34 ~ 27.09MgO
5. 92 ~6. 54Al
2
O
3
17. 32 ~22
24FeO
3. 86 ~7. 35MnO
and ingredient of refining slag sample for ladle top slag with adding modifying agent is (/% ) 34.36 ~ 40. 43CaO
7. 69 ~11.47SiO
2
6. 42 ~7. 31MgO
8.31 ~ 25. 54Al
2
O
3
11.94 ~ 20. 78FeO
2. 17 ~ 2. 63MnO; with using ladle top slag modification treatment
the actual activity coefficient a
(FeO)
in slag is less than that in equilibrium with dissolved oxygen in steel led to oxygen diffusion from steel to slag through the interface of metal-slag
thus to lower the activity of oxygen in liquid
obviously improve the cleanliness of liquid and decrease the amount and size of inclusions in casting slab
and markedly reduce the nozzle clogging occurrence. Besides
although the decrease of a
(FeO)
in slag is small
whereas the activity of oxygen in liquid decreases significantly.