Effect of Ingot Heating and Forged Products Heat Treatment Process on Banded-Structure of Φ540 mm Bar of Steel 18CrNiMo7-6
|更新时间:2026-01-21
|
Effect of Ingot Heating and Forged Products Heat Treatment Process on Banded-Structure of Φ540 mm Bar of Steel 18CrNiMo7-6
Special SteelVol. 36, Issue 2, Pages: 62-63(2015)
作者机构:
抚顺特殊钢股份有限公司技术中心,抚顺,113001
作者简介:
基金信息:
DOI:
CLC:
Received:08 October 2014,
Online First:24 August 2022,
Published:24 August 2015
稿件说明:
移动端阅览
刘金鑫, 赵敏, 冯桂萍, et al. Effect of Ingot Heating and Forged Products Heat Treatment Process on Banded-Structure of Φ540 mm Bar of Steel 18CrNiMo7-6[J]. Special Steel, 2015, 36(2): 62-63.
DOI:
刘金鑫, 赵敏, 冯桂萍, et al. Effect of Ingot Heating and Forged Products Heat Treatment Process on Banded-Structure of Φ540 mm Bar of Steel 18CrNiMo7-6[J]. Special Steel, 2015, 36(2): 62-63.DOI:
Effect of Ingot Heating and Forged Products Heat Treatment Process on Banded-Structure of Φ540 mm Bar of Steel 18CrNiMo7-6
0.0129N)的生产流程为60 t UHP EAF-LF-VD-12.5 t铸锭工艺。试验研究了钢锭加热工艺(1200~1220℃
7-8 h~13-15 h)
锻材完全退火(900℃ 12 h
≤80℃/h至650℃50 h
空冷)、等温退火(900℃ 12 h
空冷至650℃50 h
空冷)和正火(900℃ 12 h
空冷)工艺对Φ540 mm锻材带状组织的影响。结果表明
钢锭1200~1220℃ 7-8 h加热
锻材经完全退火、等温退火或正火处理后其带状级别分别为4.0
3.5和3.0
钢锭经1200~1220℃ 13-15 h加热
锻材经正火处理后其带状级别为2.5
为最佳工艺。
Abstract
Process flowsheet of test heavy gear steel 18CrNiMo7-6 (/% : 0.165C
0.59Mn
0.24Si
0.006S
0.008P
1.56Ni
1.71Cr
0.28Mo
0.034Al
0.0129N) is 60 t UHP EAF-LF-VD-12.5 t ingot casting process. The effect of ingot heating process (1200-1220 °C
7-8 〜13-15 h)
forged product complete annealing (900 °C 12 h
with ≤ 80 °C/h slow cooling to 650 °C 50 h
air cooling)
isothermal annealing (900 °C 12 h
air cooling to 650 °C 50 h
air cooling) and normalizing (900 °C 12 h
air cooling) process on banded structure of Φ540 mm forged bar has been tested and studied. Results show that as ingot heating at 1200-1220 °C for 7-8 h
the rating of banded-structure of forged bar by complete annealing
isothermal annealing or normalizing process is respectively 4.0
3.5 and 3.0
while as ingot heating at 1200-1220 °C for 13-15 h
then normalized
the rating of banded-structure of forged bar is 2.5