Effect of Ingredient on Viscosity of 100 t LF High Basicity Refining Slag and Desulphurization of steel TC80
|更新时间:2026-01-21
|
Effect of Ingredient on Viscosity of 100 t LF High Basicity Refining Slag and Desulphurization of steel TC80
Special SteelVol. 37, Issue 1, Pages: 43-46(2016)
作者机构:
1. 江西理工大学冶金与化学工程学院,赣州,341000
2. 钢铁研究总院连铸技术国家工程研究中心,北京,100081
3. 天津钢铁集团有限公司炼钢二厂,天津,300301
作者简介:
基金信息:
DOI:
CLC:
Received:10 August 2015,
Online First:25 August 2022,
Published:25 August 2016
稿件说明:
移动端阅览
赵青松, 仇圣桃, 赖朝彬, et al. Effect of Ingredient on Viscosity of 100 t LF High Basicity Refining Slag and Desulphurization of steel TC80[J]. Special Steel, 2016, 37(1): 43-46.
DOI:
赵青松, 仇圣桃, 赖朝彬, et al. Effect of Ingredient on Viscosity of 100 t LF High Basicity Refining Slag and Desulphurization of steel TC80[J]. Special Steel, 2016, 37(1): 43-46.DOI:
Effect of Ingredient on Viscosity of 100 t LF High Basicity Refining Slag and Desulphurization of steel TC80
。100 t LF精炼TC80钢生产试验表明优化后精炼渣将钢水中的硫由0.020%脱至0.005%以下
脱硫率从优化前的72%提高至84%
LF精炼终点平均T[O
]
为14×10
-6
。
Abstract
The effect of ingredient of LF refining slag (/% : 37. 5 ~54. 8CaO
9. 8 ~ 18. 2SiO
2
20 ~ 30Al
2
O
3
4 ~ 10MgO
3 ~ 10CaF
2
) with basicity 3 ~5 on viscosity has been tested and studied. Results show that the effect of CaF
2
and A1
2
O
3
on viscosity of refining slag is great and the effect of basicity and MgO on viscosity of refining slag is rather minor. With increasing CaF
2
the viscosity of refining slag decreases first and then increases
with increasing A1
2
O
3
content in slag the viscosity of slag
gradually decreases ; with Al
2
0
3
content in slag being 20% and CaF
2
≥ 6% or A1
2
O
3
content being 25% and CaF
2 ≥
3%
the viscosity value of slag at 1 500 °C is less than 0. 5 Pa • s; and it is obtained by test that better basicity R and ingredient of refining slag for viscosity is 4 ~ 5R
25% ~30% Al
2
O
3
6% 〜10% MgO
3% 〜6% CaF
2
. The results of production pilot of 100 t LF refining steel TC80 show that after refining slag optimization the sulfur content in liquid decreases to less than 0. 005% from initial 0. 020%
the desulphurization ratio increases to 84% from before optimization 72% ; and the average T [O