An Analysis on Wire Breaking of Copper-Clad steel 6A during Cold-Drawing and Process Improvement
|更新时间:2026-01-21
|
An Analysis on Wire Breaking of Copper-Clad steel 6A during Cold-Drawing and Process Improvement
Special SteelVol. 40, Issue 1, Pages: 31-33(2019)
作者机构:
沙钢钢铁研究院,张家港,215625
作者简介:
基金信息:
DOI:
CLC:
Received:19 August 2018,
Online First:23 May 2022,
Published:23 May 2019
稿件说明:
移动端阅览
李皓, 郭慧英, 张宇. An Analysis on Wire Breaking of Copper-Clad steel 6A during Cold-Drawing and Process Improvement[J]. Special Steel, 2019, 40(1): 31-33.
DOI:
李皓, 郭慧英, 张宇. An Analysis on Wire Breaking of Copper-Clad steel 6A during Cold-Drawing and Process Improvement[J]. Special Steel, 2019, 40(1): 31-33.DOI:
An Analysis on Wire Breaking of Copper-Clad steel 6A during Cold-Drawing and Process Improvement
The metallurgical production flowsheet of copper-clad steel 6A (/% : 0.03 ~ 0.06C
0.02 ~ 0.05Si
0.15 ~0. 25Mn
≤0.015P
≤ 0.015S
0.02 ~0.05Al) is hot metal desulphurization- 120 t BOF-LF-140 mm x 140 mm billet casting-continuous rolling to Φ6.5 mm coil- annealing. The breaking wire of copper-clad steel 6A during cold-drawing process from Φ6.5 mm cold-drawing to Φ0.45 mm wire has been analyzed by scanning electron microscope. Results show that there are coarse spheroidized cementite clusters at center line near the fracture of Φ0. 45 mm wire. During cold-drawing process due to the hardness of pearlite higher than that of ferrite
the fine cavities initiate at tip of pearlite and with increasing drawing passes the cavities evolve as transverse ℃- shape cracks finally led to wire breaking. With decreasing carbon and manganese content in steel respectively from 0. 05% and 0.23% to 0.03% and 0.17%
decreasing overheating extent of liquid in tundish from 35 ℃ to 25 ℃ and optimizing electromagnetic stirring parameters from 250M
1. 2 Hz to 400 A
1. 2 Hz
the phenomenon of pearlite clusters at coil center is improved and the cold-drawing wire broking ratio decreases from 1. 0 times per ton steel to 0. 2 times per ton steel.