An Analysis on Unqualified T91 Steel Bar by Ultrasonic Flaw Detection and Process Improvement
|更新时间:2026-01-21
|
An Analysis on Unqualified T91 Steel Bar by Ultrasonic Flaw Detection and Process Improvement
Special SteelVol. 40, Issue 3, Pages: 8-12(2019)
作者机构:
抚顺特殊钢股份有限公司技术处,抚顺,113001
作者简介:
基金信息:
DOI:
CLC:
Received:18 October 2018,
Online First:16 May 2022,
Published:16 May 2019
稿件说明:
移动端阅览
邢国成, 刘桂江, 李涛, et al. An Analysis on Unqualified T91 Steel Bar by Ultrasonic Flaw Detection and Process Improvement[J]. Special Steel, 2019, 40(3): 8-12.
DOI:
邢国成, 刘桂江, 李涛, et al. An Analysis on Unqualified T91 Steel Bar by Ultrasonic Flaw Detection and Process Improvement[J]. Special Steel, 2019, 40(3): 8-12.DOI:
An Analysis on Unqualified T91 Steel Bar by Ultrasonic Flaw Detection and Process Improvement
The production flowsheet of test steel T91 (/% :0.10C
0.30Si
0.45Mn
0.012P
0.005S
8.90Cr
0.95Mo
0.08Nb
0.22V) is 60 t UHP EAF-AOD-LF-VD-240 mm x 240 mm bloom casting- heating and continuous rolling. The examination results of macrostructure of unqualified steel T91 Φ90 mm products by ultrasonic flaw detection show that there are center cracks and hole in bar
by metallographic analysis it is obtained that the defects have three characteristics: (1) overheating hole and cracks; (2) axial intercrystalline cracks its source at casting bloom and (3) shrinkage cavity. With the technology measures including optimizing the casting I、U and HI zone secondary cooling water amount respectively from original 28、31 and 17 L/min to 15、18 and 10 L/min
and controlling the casting bloom heating temperature
the equiaxial crystal ratio in casting bloom center increases from original 14% to more than 25%
the rating of central cracks decreases from original 2.0 to less than 0. 5
and the unqualified ratio of steel T91 products by ultrasonic flaw detection decreases from original 5% to less than 0.2%.