Surface Defects Analysis and Mechanism Research of 15CrMoG Steel Bars and Process Improvement
|更新时间:2026-01-21
|
Surface Defects Analysis and Mechanism Research of 15CrMoG Steel Bars and Process Improvement
Special SteelVol. 40, Issue 6, Pages: 1-6(2019)
作者机构:
1. 北京科技大学工程技术研究院,北京,100083
2. 山东钢铁股份有限公司莱芜分公司,莱芜,271104
作者简介:
基金信息:
DOI:
CLC:
Received:05 June 2019,
Online First:10 May 2022,
Published:10 May 2019
稿件说明:
移动端阅览
李亚强, 刘建华, 何杨, et al. Surface Defects Analysis and Mechanism Research of 15CrMoG Steel Bars and Process Improvement[J]. Special Steel, 2019, 40(6): 1-6.
DOI:
李亚强, 刘建华, 何杨, et al. Surface Defects Analysis and Mechanism Research of 15CrMoG Steel Bars and Process Improvement[J]. Special Steel, 2019, 40(6): 1-6.DOI:
Surface Defects Analysis and Mechanism Research of 15CrMoG Steel Bars and Process Improvement
It is obtained by analysis that the surface defects of the bars are formed before heating the continuous casting billet and related to the mold meniscus fluxes. Thermo-Calc software is used to calculate the solidification phase transition of 15CrMoG steel and the formation mechanism of surface defects for 15CrMoG steel bars are analyzed. The occurrence of peritectic reaction( L+δ→γ) and peritectic transformation ( δ→γ) near the solidus temperature of 15CrMoG steels lead to the uneven growth of the initial solidified shell and intensified the segregation of P and S elements at the solidification front. Uneven growth of the initial solidified shell is the primary cause of surface defects for the bars. Fine longitudinal cracks is generated in
the weakness of the shell
and grow in the place where inclusions and sulphur gathered. Surface clefts is caused by slag inclusions in casting blanks which caused by mold level fluctuation rooted in uneven growth of the initial solidified shell. By the measures including to control [C
]
0.16% ~0.17%
[S
]
≤0.005%
shielding slag basicity 1.2
slag melting point 1200℃ and viscosity 1.0Pa·s
water rate of 260 mm x 300 mm cast bloom 150 m
3
/h
and casting speed 0. 5 m/min
the non -destructive test qualified rate increases from original 45% to 98% .