Analysis on Formation of Transverse Corner Cracks of Slab of Peritectic Steel Q345D by Slab Quenching Test and Process Improvement
|更新时间:2026-01-21
|
Analysis on Formation of Transverse Corner Cracks of Slab of Peritectic Steel Q345D by Slab Quenching Test and Process Improvement
Special SteelVol. 40, Issue 5, Pages: 64-66(2019)
作者机构:
1. 河钢邯钢公司技术中心
2. 河钢邯钢公司三炼钢厂,邯郸,056015
作者简介:
基金信息:
DOI:
CLC:
Received:11 April 2019,
Online First:13 May 2022,
Published:13 May 2019
稿件说明:
移动端阅览
颜慧成, 成旭东, 巩彦坤, et al. Analysis on Formation of Transverse Corner Cracks of Slab of Peritectic Steel Q345D by Slab Quenching Test and Process Improvement[J]. Special Steel, 2019, 40(5): 64-66.
DOI:
颜慧成, 成旭东, 巩彦坤, et al. Analysis on Formation of Transverse Corner Cracks of Slab of Peritectic Steel Q345D by Slab Quenching Test and Process Improvement[J]. Special Steel, 2019, 40(5): 64-66.DOI:
Analysis on Formation of Transverse Corner Cracks of Slab of Peritectic Steel Q345D by Slab Quenching Test and Process Improvement
220 mm steel blocks were cut at the edge of quenching testing slab of peritectic steel from curving section to straightening section
and then its surface quality and microstructure is anlysized. The result shows that transverse comer cracks appear at straightening section. With the extending of strand from curving section to straightening section
ferrite film at grain boundary of austenite become thicker and clear
and the grain size of austenite is in the range of 1.0 mm to 1.5 mm. Owing to the coarse grain of austenite and thick fragile ferrite film
transverse comer cracks spread along the grain boundary of austenite. With increasing cooling water in single narrow side of mould from original 30 〜32 m
3
/h to 34 ~36 m
3
/h
and shut the side sprayer of inner arc of straightening sections