Investigation on Process and Magnetic Properties of Low- temperature Heating Common Grain-oriented Silicon Steel Slab
|更新时间:2026-01-21
|
Investigation on Process and Magnetic Properties of Low- temperature Heating Common Grain-oriented Silicon Steel Slab
Special SteelVol. 40, Issue 5, Pages: 31-36(2019)
作者机构:
1. 技术中心
2. 冷轧硅钢厂,
作者简介:
基金信息:
DOI:
CLC:
Received:11 January 2019,
Online First:12 May 2022,
Published:12 May 2019
稿件说明:
移动端阅览
董爱锋, 侯鹏飞, 张文康. Investigation on Process and Magnetic Properties of Low- temperature Heating Common Grain-oriented Silicon Steel Slab[J]. Special Steel, 2019, 40(5): 31-36.
DOI:
董爱锋, 侯鹏飞, 张文康. Investigation on Process and Magnetic Properties of Low- temperature Heating Common Grain-oriented Silicon Steel Slab[J]. Special Steel, 2019, 40(5): 31-36.DOI:
Investigation on Process and Magnetic Properties of Low- temperature Heating Common Grain-oriented Silicon Steel Slab
The investigation was carried out on the process of 0. 30mm grain-oriented silicon steel (/% :0.03 ~ 0.05C、3.0~3.2Si、0.18〜0.24Mn、0.005 ~0.012S、0.006 ~0.011N、0.012 ~0. 024Als、0. 4 ~ 0. 55Cu) produced by low-temperature slab heating technology
in which the inhibitor of Cu
2
S + AIN was used and the two-stage cold rolling technology with completing decarburization in the intermediate thickness of cold sheet was used too. It is proved that when the heating temperature is 1220 〜1300℃,the magnetic induction increases as well as the core loss decreases with increasing Als and N in the range of Als (/% ) 0. 01 ~ 0. 022 and N (/% ) 0. 007 ~ 0. 011
and the ratio of qualified products is higher. The second cold rolling rate within 55% -60% (i. e. the thickness after first rolling being 0.65 ~0.70 mm) guarantees the uniform primary grains and proper quantities of Goss crystal nucleus. Temperature
time and thickness affect on decarburation remarkably
while the effect of atmosphere and temperature of water for adding wet is light. In addition
the recovery annealing make for little contribution to improve magnetic properties. The most proper process is heating at 1290 ℃
hot rolling at 1160 °C
finishing temperature at 930 ~ 960 °C
second cold rolling rate within 55% ~ 60%
intermediate decarburization temperature at 840 ~ 850°C
water temperature for adding wet at 65 ℃
annealing atmosphere with 20% H
2
+ 80% N
2
annealing for 8 〜9 minutes based on thickness
and the recovery annealing process can be removed.