Pilot Production on Dephosphorization and Carbon- Guaranteed Technology for 120 t Converter by Semi-Steel Steelmaking
|更新时间:2026-01-21
|
Pilot Production on Dephosphorization and Carbon- Guaranteed Technology for 120 t Converter by Semi-Steel Steelmaking
Special SteelVol. 41, Issue 6, Pages: 32-35(2020)
作者机构:
1. 攀钢集团研究院有限公司,钒钛资源综合利用国家重点实验室,攀枝花,617000
2. 攀钢集团攀枝花钢机有限公司提飢炼钢厂,攀枝花,617067
作者简介:
基金信息:
DOI:
CLC:
Received:22 May 2020,
Online First:07 May 2022,
Published:07 May 2020
稿件说明:
移动端阅览
陈均, 李盛, 周明佳, et al. Pilot Production on Dephosphorization and Carbon- Guaranteed Technology for 120 t Converter by Semi-Steel Steelmaking[J]. Special Steel, 2020, 41(6): 32-35.
DOI:
陈均, 李盛, 周明佳, et al. Pilot Production on Dephosphorization and Carbon- Guaranteed Technology for 120 t Converter by Semi-Steel Steelmaking[J]. Special Steel, 2020, 41(6): 32-35.DOI:
Pilot Production on Dephosphorization and Carbon- Guaranteed Technology for 120 t Converter by Semi-Steel Steelmaking
According to issue of increasing cost and decreasing liquid quality by BOF recarburization process to melt medium and high carbon steel using semi-steel at Pan Gang
the chemical thermal compensating process by increasing silicon content of semi-steel is adopted
and based on dephosphorization thermodynamics in BOF and enrichment regularity of phosphor in slag
it is obtaind that enrichment phase of phosphor in slag is 2CaO • SiO
2
. By using technologic measures such as fast slagging
reduce tapping temperature
it is obtained that the enrichment phase of phosphor in slag is increased
which improve the dephosphorization effect. Results of test indicate that the new thermal compensating process improves the thermal resource of semi-steel as well as shorten the slag forming time from 4. 1 min to 2. 5 min
and the average carbon content of steel at endpoint is of BOF 0.18%
it is obt
aind that temperature is 1653 °C
TFe content of slag is average reduced by 2. 81 percent point
phosphor content of steel is all less than 0.015% .