Effect of Timing of Titanium Adjustment in 210 t RH Refining Process on Cleanliness of IF Steel
|更新时间:2026-01-21
|
Effect of Timing of Titanium Adjustment in 210 t RH Refining Process on Cleanliness of IF Steel
Special SteelVol. 42, Issue 6, Pages: 25-28(2021)
作者机构:
1. 吉林电子信息职业技术学院,吉林,132021
2. 通化钢铁股份公司技术中心,通化,134003
作者简介:
基金信息:
DOI:
CLC:
Received:12 April 2021,
Online First:03 January 2022,
Published:03 January 2021
稿件说明:
移动端阅览
吕国成, 包丽明, 朱金禄. Effect of Timing of Titanium Adjustment in 210 t RH Refining Process on Cleanliness of IF Steel[J]. Special Steel, 2021, 42(6): 25-28.
DOI:
吕国成, 包丽明, 朱金禄. Effect of Timing of Titanium Adjustment in 210 t RH Refining Process on Cleanliness of IF Steel[J]. Special Steel, 2021, 42(6): 25-28.DOI:
Effect of Timing of Titanium Adjustment in 210 t RH Refining Process on Cleanliness of IF Steel
Through 3 heats IF steel of 210 t RH refining process test
the effect of titanium-adjusted time on cleanliness of IF steel in RH refining process is studied by scanning electron microscopy. The results indicate that titanium adjustment after adding aluminum for 2
4 and 6 min
the average N content in molten steel at RH end is 26. 7 x 10
-6
23. 6 x 10
-6
and 27. 4 x 10
-6
respectively. When the oxygen blowing amount for heating
the oxygen consumption is 30 〜40 m
3
and the average initial oxygen content in liquid of RH is 579 x 10
-6
the T[O
]
is 70. 3 x 10
-6
at the RH end; When the oxygen blowing amount for heating
the oxygen consumption is 75 ~ 90 m
3
and the average ar
rival oxygen of RH is 669 x 10
-6
the T[O
]
is 109. 2 x 10
-6
at the RH end. The T[O
]
at the RH end shows an increase trend with the increase of oxygen activity before adding aluminum. The quantity density of inclusions with 5μm equivalent diameter in steel is 9. 32 /mm
2
when adjusted Ti alloy after adding aluminum 6 min