Effect of Heat Treatment on Microstructures and Properties of 40CrNiMoA Steel Plate Welded Joint
|更新时间:2026-01-21
|
Effect of Heat Treatment on Microstructures and Properties of 40CrNiMoA Steel Plate Welded Joint
Special SteelVol. 43, Issue 4, Pages: 95-99(2022)
作者机构:
1. 天津职业技术师范大学天津市高速切削与精密加工重点实验室,天津,300222
2. 中国科学院金属研究所,沈阳,110016
3. 天津重型装备工程研究有限公司,天津,300457
作者简介:
基金信息:
DOI:
CLC:
Online First:21 August 2022,
Published:21 August 2022
稿件说明:
移动端阅览
刘艳梅, 陈静, 王铁钢, et al. Effect of Heat Treatment on Microstructures and Properties of 40CrNiMoA Steel Plate Welded Joint[J]. Special Steel, 2022, 43(4): 95-99.
DOI:
刘艳梅, 陈静, 王铁钢, et al. Effect of Heat Treatment on Microstructures and Properties of 40CrNiMoA Steel Plate Welded Joint[J]. Special Steel, 2022, 43(4): 95-99.DOI:
Effect of Heat Treatment on Microstructures and Properties of 40CrNiMoA Steel Plate Welded Joint
本文研究了调质工艺对40CrNiMoA钢板焊接接头显微组织及力学性能的影响。试验结果表明,经 830 - 870 °C +550 - 650 °C 调质处理后
40CrNiMoA钢3 mm板90 A 10 V焊接接头的焊缝区、热影响区、母材区的硬度差异显著减小,形成了回火索氏体组织。调质处理温度越高,焊接接头的焊缝区、热影响区与母材区的组织越 均匀
且组织中的碳化物颗粒尺寸增大。40CrNiMoA钢焊接板经850 Y油淬
600 X.回火后,具有较高的强度(905 MPa)和塑性(13. 5% ),综合力学性能最优。
Abstract
Effect of quenching and tempering process on the microstructure and mechanical properties of 40CrNiMoA steel welded joints was studied in this paper. The test results indicated that by quenching + tempering at 830 ~ 870 °C + 550 - 650 °C the 40CrNiMoA steel 3 nun plate at 90A 10V welded joint hardness difference between weld zone
heat affected zone
and base metal zone is reduced significantly
and tempered sorbite structure is formed. The higher quenching and tempering temperature
the more uniform microstructure among the weld zone
heat affected zone and base metal of welded joint
and the cementite particle grew up in structure. The 40CrNiMoA steel welded joint after oil quenching at 850°C and tempering at 600 勾 has higher strength (905 MPa) and plasticity (13. 5% ). In this case