Effect of Aging Treatment on Mechanical Properties and Microstrure of 05Crl7Ni4Cu4Nb Martensitic Precipitation Hardening Stainless Steel
|更新时间:2026-01-21
|
Effect of Aging Treatment on Mechanical Properties and Microstrure of 05Crl7Ni4Cu4Nb Martensitic Precipitation Hardening Stainless Steel
Special SteelVol. 42, Issue 5, Pages: 85-88(2021)
作者机构:
1. 太原钢铁(集团)有限公司先进不锈钢材料国家重点实验室,太原,030003
2. 山西太钢不锈钢股份有限公司技术中心,太原,030003
作者简介:
基金信息:
DOI:
CLC:
Online First:02 February 2023,
Published:02 February 2021
稿件说明:
移动端阅览
卫争艳, 徐梅, 谭国华. Effect of Aging Treatment on Mechanical Properties and Microstrure of 05Crl7Ni4Cu4Nb Martensitic Precipitation Hardening Stainless Steel[J]. Special Steel, 2021, 42(5): 85-88.
DOI:
卫争艳, 徐梅, 谭国华. Effect of Aging Treatment on Mechanical Properties and Microstrure of 05Crl7Ni4Cu4Nb Martensitic Precipitation Hardening Stainless Steel[J]. Special Steel, 2021, 42(5): 85-88.DOI:
Effect of Aging Treatment on Mechanical Properties and Microstrure of 05Crl7Ni4Cu4Nb Martensitic Precipitation Hardening Stainless Steel
strength and hardness of martensitic precipitation hardening stainless steel 05Cr17Ni4Cu4Nb solid solution at 1 040 °C and aged at 480 ~ 620 °C for 5 h have been tested and studied. The results show that with the increasing aging temperature
the descomposition of martensitic matrix structrue gradually and the precipitation of carbide decrease. During the aging treatment
with increasing aging temperature the copper-rich phase is precipitaed as a sphere at first and then gradually developed to oval and rod shape
the size of precipitates are increased
the number decreased and the coherent interface with the matrix disappears
the stengthening effect decreases. With solution-treated at 1 040 °Cand aged at 480 °C for 5 h
the HRC hardness number of 05Crl7Ni4Cu4Nb steel is 44.3
to meet the requirement of product HRC hardness number 43.