Static Recrystallization of Double-Pass Compressed Austenite of steel 30CrMo 60 mm Casting Slab

Guo Jinxing , Bao Siqian , Peng Lian , Tang Shunqi   

  1. Key Laboratory for Ferrous Metallurgy and Resources Utilization of Ministry of Education,Wuhan University of Science and Technology, Wuhan 430081
  • Received:2015-10-08 Online:2016-04-01 Published:2022-08-08

30CrMo钢60 mm连铸板坯双道次压缩的奥氏体静态再结晶

郭金星,鲍思前,彭 联,汤顺启   

  1. 武汉科技大学钢铁冶金及资源利用省部共建教育部重点实验室,武汉 430081
  • 作者简介:郭金星(1989-),男,硕士研究生,2011年武汉科技大学(本科)毕业,中高碳钢组织和性能控制。
  • 基金资助:
    湖北省自然科学基金项目(2014CFB819)资助

Abstract: The static recrystallization behavior of steel 30CrMo 60 mm casting slab in interval between double-pass of hot deformation has been tested and studied by Thermecmastor-Z thermal simulator and double-pass compressed method to analysis the effect of temperature (1000 ~ 1150℃),deformation (0.1-0.22) , strain rate ( 0.1-10 s-1) and inlerval between passes (1-80 s) on static recrystallization. Results show that the static recrystallization of steel 30CrMo is improved with increasing temperature, deformation, strain rate and interval between passes ; the static recrystallization activation energy of steel 30CrMo is 184.45 kJ/mol ; a static recrystallization kinetic model is established based on experimental data and the predicted data better meet the experimental data.

Key words: Steel 30CrMo, 60 mm Casting Slab, Double-Pass Compression, Static Recrystallization, Kinetic Model

摘要: 在Thermecmastor-Z热模拟机上利用双道次压缩方法实验研究30CrMo钢60 mm连铸板坯高温变形道次间隔时间内的静态再结晶行为,分析温度(1000~1150℃),变形量(0.1~0.22),变形速率(0.1~10 s-1)以及道次间隔时间(1~80 s)对其静态再结晶的影响。结果表明,温度、变形量、变形速率及道次间隔时间的增加都会促进30CrMo钢的静态再结晶;30CrMo钢的静态再结晶激活能为184.45 kJ/mol;根据实验数据建立了静态再结晶动力学模型,模型预测结果与实验结果吻合较好。

关键词: 30CrMo钢, 60 mm连铸板坯, 双道次压缩, 静态再结晶, 动力学模型