Effect of Charging Structure on Electric Power Consumption of a 50 t Arc furnace at Shijiazhuang Iron and Steel
|更新时间:2026-01-21
|
Effect of Charging Structure on Electric Power Consumption of a 50 t Arc furnace at Shijiazhuang Iron and Steel
Special SteelVol. 26, Issue 1, Pages: 55-56(2005)
作者机构:
北京科技大学冶金学院,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:20 July 2004,
Online First:24 May 2023,
Published:24 May 2005
稿件说明:
移动端阅览
李峰, 曹立国, 李士琦. Effect of Charging Structure on Electric Power Consumption of a 50 t Arc furnace at Shijiazhuang Iron and Steel[J]. Special Steel, 2005, 26(1): 55-56.
DOI:
李峰, 曹立国, 李士琦. Effect of Charging Structure on Electric Power Consumption of a 50 t Arc furnace at Shijiazhuang Iron and Steel[J]. Special Steel, 2005, 26(1): 55-56.DOI:
Effect of Charging Structure on Electric Power Consumption of a 50 t Arc furnace at Shijiazhuang Iron and Steel
The statistics data of charging structure as well as scrap
hot metal and electric pawer consumption per ton steel of two batches 1249 heats of a 50t arc furnace at Shijiazhuang Iron and Steel have been analyzed by using Statistics Package for Social Science (SPSS) software and iron-steel ratio to describe binary charging structure. The results showed that with charging iron-steel ratio increasing the electric power consumption per ton steel decreased. And the quantity relation between specific electric power consumption per ton steel (SEC)and iron-steel proportion (ISP)for two batches was obtained by curve regressive method
that is SEC= 402 e
-0.59ISP
for first batch and SEC= 327 e
-0.49ISP
for second batch
as iron-steel proprotein increased from 0.56 to 1. 11
the electric pawer consumption per ton steel decreased by 53 kWh/t.