Process Practice for Production of Caterpillar Track Steel 35MnBM by 90 t EAF-LF(VD)-CC-CR Flow Sheet
|更新时间:2026-01-21
|
Process Practice for Production of Caterpillar Track Steel 35MnBM by 90 t EAF-LF(VD)-CC-CR Flow Sheet
Special SteelVol. 29, Issue 2, Pages: 58-59(2008)
作者机构:
东北特钢集团北满特殊钢有限责任公司,齐齐哈尔,161041
作者简介:
基金信息:
DOI:
CLC:
Online First:20 January 2023,
Published:20 January 2008
稿件说明:
移动端阅览
朱志欣李艾王秀兰. Process Practice for Production of Caterpillar Track Steel 35MnBM by 90 t EAF-LF(VD)-CC-CR Flow Sheet[J]. Special Steel, 2008, 29(2): 58-59.
DOI:
朱志欣李艾王秀兰. Process Practice for Production of Caterpillar Track Steel 35MnBM by 90 t EAF-LF(VD)-CC-CR Flow Sheet[J]. Special Steel, 2008, 29(2): 58-59.DOI:
Process Practice for Production of Caterpillar Track Steel 35MnBM by 90 t EAF-LF(VD)-CC-CR Flow Sheet
φ70 mm products of caterpillar track steel 35MnBM(0.35C
1.25Mn
0.0018B
0.029Al
0.09V)was produced by 90 t electric arc fumace-LF(VD)refining -240 mm×240 mm billet concasting - continuous rolling process at Beiman Special Steel. With VD treatment and whole period shield casting practice the[N] was ≤78× 10-6
the rating of non- metallic inclusions in steel was 0~2
no hair crack was detected and the grain size
structure and hardenability of steel all met the requirement of standard