An Analysis on Cold Upsetting Crack of 0. 45 C Steel 010 mm Products and Process Improved Measures
|更新时间:2026-01-21
|
An Analysis on Cold Upsetting Crack of 0. 45 C Steel 010 mm Products and Process Improved Measures
Special SteelVol. 30, Issue 1, Pages: 50-51(2009)
作者机构:
1. 东北大学材料与冶金学院,沈阳,110004
2. 抚顺新钢铁有限责任公司,抚顺,113001
3. 北京科技大学,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:16 July 2008,
Online First:30 November 2022,
Published:30 November 2009
稿件说明:
移动端阅览
李勇, 战东平, 韩作宽, et al. An Analysis on Cold Upsetting Crack of 0. 45 C Steel 010 mm Products and Process Improved Measures[J]. Special Steel, 2009, 30(1): 50-51.
DOI:
李勇, 战东平, 韩作宽, et al. An Analysis on Cold Upsetting Crack of 0. 45 C Steel 010 mm Products and Process Improved Measures[J]. Special Steel, 2009, 30(1): 50-51.DOI:
An Analysis on Cold Upsetting Crack of 0. 45 C Steel 010 mm Products and Process Improved Measures
According to analysis on cold upsetting crack of 0. 45C steel φ10 mm rolled products produced by 40 t LD- ladle argon blowing- CC- high speed rod mill process flow sheet at New Fushun Steel
it was obtained that the inclusions Al
2
O
3
MnS and the lamellar pearlite in steel were main reason to form cold upsetting crack. With decreasing the sulphur content in charge
decreasing [S]from 0. 029% to 0. 020%,controlling LD end [C
]
and decreasing end [O
]
spheroidizing annealing rolled products to increase elongation of steel from original 21. 6% to 30. 4%
the formation of cold upsetting crack was avoided.