Influence of Finishing Forging Temperature and Forging Ratio on Precipitation of Ferrite in Non-Quenched and Tempered Bainitic Steel
|更新时间:2026-01-21
|
Influence of Finishing Forging Temperature and Forging Ratio on Precipitation of Ferrite in Non-Quenched and Tempered Bainitic Steel
Special SteelVol. 30, Issue 1, Pages: 66-67(2009)
作者机构:
上海大学材料科学勺匸程学院,上海,200072
作者简介:
基金信息:
DOI:
CLC:
Received:16 July 2008,
Online First:30 November 2022,
Published:30 November 2009
稿件说明:
移动端阅览
彭金明, 汪宏斌, 罗毅, et al. Influence of Finishing Forging Temperature and Forging Ratio on Precipitation of Ferrite in Non-Quenched and Tempered Bainitic Steel[J]. Special Steel, 2009, 30(1): 66-67.
DOI:
彭金明, 汪宏斌, 罗毅, et al. Influence of Finishing Forging Temperature and Forging Ratio on Precipitation of Ferrite in Non-Quenched and Tempered Bainitic Steel[J]. Special Steel, 2009, 30(1): 66-67.DOI:
Influence of Finishing Forging Temperature and Forging Ratio on Precipitation of Ferrite in Non-Quenched and Tempered Bainitic Steel
Influence of finishing temperature 810 ~960 ℃ and forging ratio 3 -6 on precipitation of ferrite in bainitic steel-0. 16C
0.91 Si
1.98Mnt 1.03Cr
0. 17Mo
0. 065V
0. 001 Ti has been studied. Results showed that the critical temperature of phase transformation for austenite to ferrite increased by deformation of the bainitic steel during forging; with forging finishing at 810 ~ 820 ℃. the defbnnation induced ferrite precipitation occurred in steel and with increasing forging ratio from 3 to 6
the volume fraction of ferrite in steel increased from 1. 8% to 9. 6% accompanied acic ular ferrite evolving to massive ferrite; and with forging finishing at 940 -960 °C
most of ferrite in steel was acicular
with increasing forging ratio from 3 to 6 the volume fraction of ferrite in steel dec revised from 3. 0% to 0. 6% .