Behavior of Thermal Deformation of High Quality Non-Quenched-Tempered Steel YF45MnVS for Automobile
|更新时间:2026-01-21
|
Behavior of Thermal Deformation of High Quality Non-Quenched-Tempered Steel YF45MnVS for Automobile
Special SteelVol. 31, Issue 6, Pages: 56-58(2010)
作者机构:
北京科技大学冶金与生态工程学院,北京,100083
作者简介:
基金信息:
DOI:
CLC:
Received:28 June 2010,
Online First:28 October 2022,
Published:28 October 2010
稿件说明:
移动端阅览
邵肖静, 邓小玄, 崔睿, et al. Behavior of Thermal Deformation of High Quality Non-Quenched-Tempered Steel YF45MnVS for Automobile[J]. Special Steel, 2010, 31(6): 56-58.
DOI:
邵肖静, 邓小玄, 崔睿, et al. Behavior of Thermal Deformation of High Quality Non-Quenched-Tempered Steel YF45MnVS for Automobile[J]. Special Steel, 2010, 31(6): 56-58.DOI:
Behavior of Thermal Deformation of High Quality Non-Quenched-Tempered Steel YF45MnVS for Automobile
The isothermal compression test for Φ8 mm specimen of steel YF45MnVS ( % : 0. 48C
0. 45Si
1. 36Mn
0. 009P
0. 043S
0. 086V) cut from 200 mm x 200 mm cast bloom with single pass strain rate 10
-2
〜10
1
s
-1
and strain 10% 〜50% at 950 〜1 200 °C has been carried out by using Gleeble-1500 thermo-mechanical simulator. Results show that low strain rate and large strain are favorable to the occurrence of dynamic recrystallization of test steel. The calculated dynamic recrystallized activation energy of the steel YF45MnVS at 950 〜1 200 ℃ is 299. 55 kJ/mol.