Effect of Heat Treatment on Structure and Properties of Annealed Cold Rolled Sheet of Martensitic Stainless Steel 5Cr15MoV
|更新时间:2026-01-21
|
Effect of Heat Treatment on Structure and Properties of Annealed Cold Rolled Sheet of Martensitic Stainless Steel 5Cr15MoV
Special SteelVol. 32, Issue 2, Pages: 66-68(2011)
作者机构:
宝山钢铁股份有限公司技术中心,上海,200431
作者简介:
基金信息:
DOI:
CLC:
Received:23 November 2010,
Online First:10 November 2022,
Published:10 November 2011
稿件说明:
移动端阅览
秦斌. Effect of Heat Treatment on Structure and Properties of Annealed Cold Rolled Sheet of Martensitic Stainless Steel 5Cr15MoV[J]. Special Steel, 2011, 32(2): 66-68.
DOI:
秦斌. Effect of Heat Treatment on Structure and Properties of Annealed Cold Rolled Sheet of Martensitic Stainless Steel 5Cr15MoV[J]. Special Steel, 2011, 32(2): 66-68.DOI:
Effect of Heat Treatment on Structure and Properties of Annealed Cold Rolled Sheet of Martensitic Stainless Steel 5Cr15MoV
The effect of normalizing treatment at 950 〜1 200 °C on mechanical property and 5% NaCl salt spray corrosion resistance at 35℃ of 2 mm annealed cold rolled. sheet of steel 5Crl5MoV (% : 0. 50C
14. 16Cr
0. 66Mo
0. 12 V
0. 39Ni) has been studied. Results show that as normalized at 950 ~ 1 150℃ with increasing temperature the carbide in steel reduces
while the hardness of steel increases; as normalized at 1 200 °C there is definite amount of residual austenite in matrix of steel led to a decrease of hardness of steel ; and as normalized temperature is higher than 1 100 °C the corrosion resistance of steel decreases easily to occur grain-boundary attack. Therefore
it is available to get higher hardness and better corrosion resistance by normalizing at 1 135 ℃.