S and Si content in ultra-pure austenite steel 005Cr25Ni20 (% :24 ~26Cr
19 〜22Ni) are very low i. e. (%) :≤0. 010C
≤0. 010S
≤0. 010P and W≤0. 15 Si
the steel is smelted by 3 t vacuum induction furnace 4- vacuum consumption remelting furnace steelmaking process. With using quality pure iron (% : 0. 009C
0. 035Si
0. 001 2S
0. 004 5P)
high pure chromium iron (%: 0. 010 - 0. 021C
0. 11 - 0. 13Si
0. 002 5 ~0. 005 OS
0. 001 5 ~0. 005 OP) and Ni-plate (Ni399%)
adding Al
metal Ca
Ni-Mg for deoxidation during vacuum induction smelting
and whole process computer control vacuum consumption remelting speed
the chemical composition of finished products of steel is (% :)
0. 005 〜0.007C
0. 33 〜0. 34Mn
0. 03 -0. 04Si
0. 001 〜0.002S
0. 004 〜 0. 005P
24. 34 〜24. 62Cr
21. 20 〜21.25Ni to meet the technical requirement
and the oxygen content in steel- (12 ~ 22) x 10
-6
is lower than in steel by ESR process- (30 ~ 80) x 10