Optimization of Process for 300 Series Cr-Ni Austenitic Stainless Steel Melted by Consteel Arc Furnace-AOD Two Step Method
|更新时间:2026-01-21
|
Optimization of Process for 300 Series Cr-Ni Austenitic Stainless Steel Melted by Consteel Arc Furnace-AOD Two Step Method
Special SteelVol. 33, Issue 1, Pages: 30-31(2012)
作者机构:
1. 中冶华天工程技术有限公司,马鞍山,243005
2. 冶金工业规划研究院,北京,100711
作者简介:
基金信息:
DOI:
CLC:
Received:11 July 2011,
Online First:20 September 2022,
Published:20 September 2012
稿件说明:
移动端阅览
高玉来, 李闯. Optimization of Process for 300 Series Cr-Ni Austenitic Stainless Steel Melted by Consteel Arc Furnace-AOD Two Step Method[J]. Special Steel, 2012, 33(1): 30-31.
DOI:
高玉来, 李闯. Optimization of Process for 300 Series Cr-Ni Austenitic Stainless Steel Melted by Consteel Arc Furnace-AOD Two Step Method[J]. Special Steel, 2012, 33(1): 30-31.DOI:
Optimization of Process for 300 Series Cr-Ni Austenitic Stainless Steel Melted by Consteel Arc Furnace-AOD Two Step Method
改进的工艺为60 t Consteel电弧炉+140 t EAF-150 t AOD流程。60 t Consteel EAF用低镍高磷生铁
其终点[P
]
为≤250×10
-6
加上85 t EAF终点[P
]
450×10
-6
的钢水
使AOD精炼前的[P
]
≤360×10
-6
。新工艺冶炼周期缩短10~30 min
钢水磷含量从450×10
-6
降至360 X 10
-6
以下
提高了不锈钢产品质量
并显著降低了生产成本。
Abstract
The original process to produce 300 series stainless steel at steel works is 140 t EAF-150 t AOD two step method
and with charging partial low nickel high phosphorus pig iron
the EAF end [ P
]
is 450 x 10
-6
. In order to decrease EAF end [P
]
the improved process-60 t Consteel arc furnace + 140 t EAF-150 t AOD flow sheet is adopted. With charging low nickel high phosphorus pig iron in 60 t Consteel arc furnace
its end [ P
]
is ≤250 x 10
-
6
mixing with 85 t end [ P
]
450 x 10
-6
EAF liquid
the [P
]
before AOD refining is ≤360 x 10
-6
. With using new developed process
the tap-to-tap time reduce by 10 ~ 30 min
the phosphorus content in liquid decreases to less than 360 x 10
-6
from original 450 x 10
-6
the product quality of stainless-steel increases and the production cost decreases obviously.